MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

(Viewing data as-entered. Click here to return)
Hexcel® HexPly® M65 Bismaleimide Resin, Carbon Fabric Form
Categories: Polymer; Thermoset; Bismaleimide (BMI)

Material Notes: Fibers: T300-3K, AS4C-3K

Information provided by HexCel

Key Words: BMI
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.52 g/ccLaminate
Filler Content 51.0 %Laminate Fiber Volume
Volatiles <= 2.0 %Prepreg
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength, Yield 744 MPa
@Temperature 23.0 °C
T300; Fill Tension; (AMB)
 841 MPa
@Temperature 23.0 °C
AS4C; Fill Tension; (AMB)
Tensile Modulus 55.8 GPa
@Temperature 23.0 °C
 56.3 GPa
@Temperature 23.0 °C
Flexural Yield Strength 520 MPa
@Temperature 177 °C
AS4C; Fill Flexure; Wet condition
 552 MPa
@Temperature 177 °C
T300; Fill Flexure; Wet condition
 710 MPa
@Temperature 232 °C
AS4C; Fill Flexure;
 758 MPa
@Temperature 232 °C
T300; Fill Flexure; AMB
 917 MPa
@Temperature 23.0 °C
 1041 MPa
@Temperature 23.0 °C
Flexural Modulus 51.3 GPa
@Temperature 177 °C
T300; Fill Flexure; Wet condition
 52.0 GPa
@Temperature 177 °C
AS4C; Fill Flexure; Wet condition
 54.0 GPa
@Temperature 232 °C
T300; Fill Flexure; AMB
 54.0 GPa
@Temperature 232 °C
AS4C; Fill Flexure;
 56.8 GPa
@Temperature 23.0 °C
 57.0 GPa
@Temperature 23.0 °C
Compressive Yield Strength 408 MPa
@Temperature 177 °C
AS4C; Fill Compression; Wet condition
 438 MPa
@Temperature 177 °C
T300; Fill Compression; Wet condition
 510 MPa
@Temperature 232 °C
T300; Fill Compression; AMB
 531 MPa
@Temperature 232 °C
AS4C; Fill Compression;
 786 MPa
@Temperature 23.0 °C
 889 MPa
@Temperature 23.0 °C
Compressive Modulus 8.18 GPa
@Temperature 177 °C
T300; Fill Compression; Wet condition
 8.40 GPa
@Temperature 23.0 °C
Shear Modulus 1.40 GPa
@Temperature 177 °C
T300; In Plane; Wet condition
 1.60 GPa
@Temperature 177 °C
AS4C; In Plane; Wet condition
 2.70 GPa
@Temperature 232 °C
T300; In Plane; AMB
 2.70 GPa
@Temperature 232 °C
AS4C; In Plane
 4.50 GPa
@Temperature 23.0 °C
 4.50 GPa
@Temperature 23.0 °C
Shear Strength 34.0 MPa
@Temperature 177 °C
AS4C; Fill Short Beam; Wet condition
 39.0 MPa
@Temperature 177 °C
T300; Fill Short Beam; Wet condition
 50.0 MPa
@Temperature 232 °C
AS4C; Fill Short Beam
 54.0 MPa
@Temperature 232 °C
T300; Fill Short Beam; AMB
 67.0 MPa
@Temperature 232 °C
AS4C; In Plane
 68.0 MPa
@Temperature 23.0 °C
 70.0 MPa
@Temperature 232 °C
T300; In Plane; AMB
 70.0 MPa
@Temperature 177 °C
AS4C; In Plane; Wet condition
 79.0 MPa
@Temperature 177 °C
T300; In Plane; Wet condition
 103 MPa
@Temperature 23.0 °C
 120 MPa
@Temperature 23.0 °C
 133 MPa
@Temperature 23.0 °C
 
Descriptive Properties
Cured Thickness per Ply (cm)0.0212Laminate
Dry Resin Content (%)40Prepreg

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Hexcel® HexPly® F650 Bismaleimide Resin
Hexcel® HexPly® F655 Bismaleimide Resin
Hexcel® HexPly® M65 Bismaleimide Resin
HOS-Technik Homide 250 Bismaleimide Resin
Vyncolit Neopreg Kinel® SK4503 S5 Aramid Reinforced Molding Compound

PHEXC016 / 98486

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.