MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

Rogers Arlon 44981R015 0.015" (0.381 mm) Uncured Silicone Rubber with Fiberglass Substrate
Categories: Polymer; Thermoset; Silicone; Silicone Rubber; Silicone, Molded, Glass Fiber Filled

Material Notes: Design/Construction:
Interleave 1: Polyethylene
Side 1: Uncured Silicone Rubber
Substrate: Style 1165 Fiberglass
Side 2: Uncured Silicone Rubber
Interleave 2: Polyethylene

UL Recognition File: E54153

Product Use: Flexible heater substrate

Appearance: Red colored, high viscosity gum on fiberglass cloth

This data represents typical values for the production material. The data should not be used to write, or in place of, material specifications.

Information provided by Arlon Silicone Technologies Division; now a part of Rogers Corporation.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.57 g/cc0.0567 lb/in³Silicone Property; Arlon SQA-TMS-024
Thickness 127 microns5.00 milSide 1; Arlon SQA-TMS-003
 127 microns5.00 milSide 2; Arlon SQA-TMS-003
 127 microns5.00 milSubstrate; Arlon SQA-TMS-003
 381 microns15.0 milOverall; Arlon SQA-TMS-003
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A 7272Silicone Property; ASTM D2240
Tensile Strength 4.83 MPa700 psiSilicone Property; ASTM D412
Elongation at Break 190 %190 %Silicone Property; ASTM D412
Peel Strength 0.614 kN/m3.50 pliBond Strength; Arlon SQA-TMS-011
 
Electrical PropertiesMetricEnglishComments
Dielectric Strength 39.4 kV/mm1000 kV/inASTM D149
 
Thermal PropertiesMetricEnglishComments
Maximum Service Temperature, Air 232 °C450 °F
Minimum Service Temperature, Air -56.7 °C-70.0 °F
UL RTI, Electrical 150 °C302 °F
UL RTI, Mechanical without Impact 150 °C302 °F
Flammability, UL94 V-0V-0
 
Processing PropertiesMetricEnglishComments
Cure Time 120 min
@Temperature 204 °C
2.00 hour
@Temperature 400 °F
Recommended Postcure Cycle
 15.0 min
@Pressure 0.345 MPa,
Temperature 121 °C
0.250 hour
@Pressure 50.0 psi,
Temperature 250 °F
Recommended Cure Cycle
Shelf Life 6.00 Month
@Temperature 21.1 °C
6.00 Month
@Temperature 70.0 °F
From date of manufacture
 
Descriptive Properties
ColorRed
 RedSubstrate
Total Product Weight (oz/yd2)18.4Arlon SQA-TMS-025

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Dow C6-350LH ELASTOMER KIT
Dow C6-180 ELASTOMER KIT
Dow 5-8601 FLUOROSILICONE LSR, KIT
Dow 3-6891 1-PART SILICONE RUBBER ABRADABLE SEALANT COMPOUND
Dow 3-6655 THERMALLY CONDUCTIVE ELASTOMER, KIT

PARL218 / 125404

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.