MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
Special Metals INCONEL® Alloy HX
Categories: Metal; Nonferrous Metal; Nickel Alloy; Superalloy

Material Notes: A nickel-chromium-iron-molybdenum alloy with outstanding strength and oxidation resistance at temperatures to 2200°F (1200°C). Matrix stiffening provided by the molybdenum content results in high strength in a solid-solution alloy having good fabrication characteristics. Used in gas turbines, industrial furnaces, heat-treating equipment, and nuclear engineering. Standard product forms are round, extruded section, flats, forging stock, plate, sheet, strip, and wire.

Data provided by the manufacturer, Special Metals.

Key Words: ASME SB-435, SB-572, SB-619, SB-622, SB-626, Boiler Code Sections III, VIII, IX, Nickel-Chromium Alloy; Werkstoff Nr. 2.4665, SAE AMS 5536, 5587, 5588, 5754, 5798, 7237; WL Nr. 2.4665; AFNOR NC 22 Fe D; NACE MR-01-75; AECMA Pr EN 2182 - 2185, UNS N06002; BS HR6, HR204; ASTM B 435, B 572, B 619, B 622, B 626, B 751
Vendors: Visit metalmen for your metals needs. Products include special chemistry, tight tolerances, custom tempers, odd dimensions/forms, and small quantities. Phone 1-800-767-9494.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Density 8.23 g/cc
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength, Ultimate 630 MPa
@Temperature 550 °C
Solution Annealed prior to test
 825 MPa
@Temperature 23.0 °C
Tensile Strength, Yield 375 MPa
@Strain 0.2 %
Solution Annealed. Value at room temperature
 210 MPa
@Strain 0.2 %,
Temperature 550 °C
Solution Annealed prior to test
Elongation at Break 42 %Solution Annealed
 48 %
@Temperature 550 °C
Solution Annealed prior to test.
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.000116 ohm-cm
Magnetic Permeability 1.011at 200 Oersted (15.9 kA/m)
 
Thermal PropertiesOriginal ValueComments
CTE, linear 13.3 µm/m-°C
@Temperature 20.0 - 100 °C
Specific Heat Capacity 0.461 J/g-°C
Thermal Conductivity 11.6 W/m-K
Melting Point 1260 - 1355 °C
Solidus 1260 °C
Liquidus 1355 °C
 
Component Elements PropertiesOriginal ValueComments
Carbon, C 0.50 - 2.5 %
Chromium, Cr 20.5 - 23 %
Cobalt, Co 0.50 - 2.5 %
Iron, Fe 17 - 20 %
Manganese, Mn <= 1.0 %
Molybdenum, Mo 8.0 - 10 %
Nickel, Ni 45 %As remainder
Phosphorus, P <= 0.040 %
Silicon, Si <= 1.0 %
Sulfur, S <= 0.030 %
Tungsten, W 0.20 - 1.0 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Special Metals INCONEL® Alloy 718
Industeel VIRGO 17.4PH 17Cr-4Ni-3Cu Precipitation Hardening Martensitic Stainless Steel (593°C - 4 hours + air cooled)
Special Metals INCONEL® Alloy X-750
Special Metals INCONEL® Alloy C-276
Special Metals INCONEL® Alloy 617

NINC52 / 17409

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.