MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

Teknor Apex Sarlink® TPV 3480N Thermoplastic Vulcanizate
Categories: Polymer; Thermoplastic; Elastomer, TPE; Thermoplastic Vulcanizate Elastomer (TPV)

Material Notes: Notes: Sarlink TPV 3480N is a high performance thermoplastic vulcanizate used in a variety of automotive, consumer and industrial applications. Sarlink TPV 3480N is a medium hardness, low density, RoHS compliant grade suitable for injection molding, blow molding and extrusion.

Availability: Asia Pacific; Europe; Latin America; North America

Features: Chemical Resistant; General Purpose; Good Adhesion; High Heat Resistant; Low Density; Medium Hardness; Low Specific Gravity

Uses: Fittings; General Purpose; Piping; Potable Water Applications

RoHS Compliance: RoHS Compliant

Agency Ratings: NSF STD-61

Form: Pellets

Processing Method: Extrusion; Injection Molding; Blow Molding; Pipe Extrusion

Information provided by Teknor Apex

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.950 g/cc0.0343 lb/in³ASTM D792
Viscosity 290 cP
@Shear Rate 206 1/s,
Temperature 200 °C
290 cP
@Shear Rate 206 1/s,
Temperature 392 °F
Shear, Capillary; ASTM D3835
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A  80
@Time 5.00 sec
80
@Time 0.00139 hour
Extruded; ISO 868
 84
@Time 5.00 sec
84
@Time 0.00139 hour
Injection Molded; ISO 868
Tensile Strength at Break 7.10 MPa1030 psiFlow; ASTM D412
 9.31 MPa1350 psiAcross Flow; ASTM D412
Tensile Strength, Yield 7.10 MPa1030 psiFlow; ASTM D412
 9.31 MPa1350 psiAcross Flow; ASTM D412
Tensile Stress at Strain  4.50 MPa
@Strain 100 %
653 psi
@Strain 100 %
Across Flow; ISO 37
 5.10 MPa
@Strain 100 %
740 psi
@Strain 100 %
Flow; ISO 37
 4.91 MPa
@Strain 100 %,
Treatment Temp. 150 °C
712 psi
@Strain 100 %,
Treatment Temp. 302 °F
Across Flow, Change in Air at 168 hr; ISO 188
 5.27 MPa
@Strain 100 %,
Treatment Temp. 135 °C
764 psi
@Strain 100 %,
Treatment Temp. 275 °F
Across Flow, Change in Air at 1000 hr; ISO 188
Elongation at Break 430 %430 %Flow; ISO 37
 680 %680 %Across Flow; ISO 37
 571 %
@Treatment Temp. 150 °C,
Time 605000 sec
571 %
@Treatment Temp. 302 °F,
Time 168 hour
Across Flow, Change in Air; ISO 188
 578 %
@Treatment Temp. 135 °C,
Time 3.60e+6 sec
578 %
@Treatment Temp. 275 °F,
Time 1000 hour
Across Flow, Change in Air; ISO 188
Tear Strength 50.8 kN/m290 pliMethod Ba, Angle (Unnicked); ISO 34-1
Compression Set  32 %
@Temperature 22.8 °C,
Time 79200 sec
32 %
@Temperature 73.0 °F,
Time 22.0 hour
ISO 815
 46 %
@Temperature 70.0 °C,
Time 79200 sec
46 %
@Temperature 158 °F,
Time 22.0 hour
ISO 815
 52 %
@Temperature 125 °C,
Time 252000 sec
52 %
@Temperature 257 °F,
Time 70.0 hour
ISO 815
 
Processing PropertiesMetricEnglishComments
Processing Temperature 182 - 221 °C360 - 430 °FInjection
Rear Barrel Temperature 177 - 216 °C350 - 420 °FInjection
Middle Barrel Temperature 177 - 216 °C350 - 420 °FInjection
Front Barrel Temperature 177 - 216 °C350 - 420 °FInjection
Nozzle Temperature 188 - 221 °C370 - 430 °FInjection
Zone 1 182 - 204 °C360 - 400 °FExtrusion
Zone 2 182 - 204 °C360 - 400 °FExtrusion
Zone 3 188 - 210 °C370 - 410 °FExtrusion
Zone 4 188 - 210 °C370 - 410 °FExtrusion
Die Temperature 193 - 216 °C380 - 420 °FExtrusion
Melt Temperature 193 - 216 °C380 - 420 °FExtrusion
Mold Temperature 10.0 - 65.6 °C50.0 - 150 °FInjection
Drying Temperature 82.2 °C180 °F
Dry Time 3.00 hour3.00 hour
Screw Speed 100 - 200 rpm100 - 200 rpmInjection
 
Descriptive Properties
AppearanceOpaque

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PTEKNQ1150 / 237641

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.