Plaskolite Optix® CA - 1000 E-2 High Impact Grade Acrylic Resin
Categories:
Polymer
;
Thermoplastic
;
Acrylic (PMMA)
;
Acrylic, Impact Modified, Molded
;
Acrylic, Optical Grade, Molded
Material Notes:
OPTIX® impact-modified grades offer 7 to 10 times the impact resistance of general purpose polymers while maintaining optical clarity.
Information provided by Plaskolite, Inc.
Vendors:
No vendors are listed for this material. Please
click here
if you are a supplier and would like information on how to add your listing to this material.
Printer friendly version
Download as PDF
Download to Excel (requires Excel and Windows)
Export data to your CAD/FEA program
Add to Folder:
My Folder
Physical Properties
Metric
English
Comments
Density
1.16
g/cc
0.0419
lb/in³
ASTM D-792
Linear Mold Shrinkage
0.0020
-
0.0060
cm/cm
0.0020
-
0.0060
in/in
ASTM D-955
Melt Flow
0.80
g/10 min
@Load 3.80 kg,
Temperature 230 °C
0.80
g/10 min
@Load 8.38 lb,
Temperature 446 °F
ASTM D-1238
Mechanical Properties
Metric
English
Comments
Tensile Strength
44.9
MPa
6510
psi
ASTM D-638
Elongation at Break
38 %
38 %
ASTM D-638
Modulus of Elasticity
1.76
GPa
255
ksi
ASTM D-638
Flexural Strength
61.3
MPa
8890
psi
ASTM D-790
Izod Impact, Notched
0.641
J/cm
@Thickness 6.35 mm
1.20
ft-lb/in
@Thickness 0.250 in
ASTM D-256
Gardner Impact
6.33
J
@Thickness 3.17 mm
4.67
ft-lb
@Thickness 0.125 in
Falling Weight; ASTM D-3029 GB
Thermal Properties
Metric
English
Comments
CTE, linear
120
µm/m-°C
66.7
µin/in-°F
ASTM D-696
Deflection Temperature at 1.8 MPa (264 psi)
80.0
°C
176
°F
ASTM D-648
Vicat Softening Point
108
°C
227
°F
ASTM D-1525
Optical Properties
Metric
English
Comments
Haze
<= 2.0 %
<= 2.0 %
ASTM D-1003
Transmission, Visible
91.7 %
91.7 %
ASTM D-1003
Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's
terms of use
regarding this information.
Click here
to view all the property values for this datasheet as they were originally entered into MatWeb.
Users viewing this material also viewed the following:
Plaskolite West Optix® CA-945 Clear Impact Modified Acrylic Resin
Plaskolite West Optix® CA-990 Impact Modified Acrylic Resin
Plaskolite West Optix® CA-1000 IG Clear High Impact Acrylic Resin
Plaskolite West Optix® CA - 900 High Impact Acrylic Resin
Plaskolite West Optix® CA - 1000 E-2 High Impact Acrylic Resin
PPLAS989 / 150546
Subscribe to Premium Services
Searches:
Advanced
•
Composition
•
Property
•
Material Type
•
Manufacturer
•
Trade Name
•
UNS Number
Other Links:
Advertising
•
Submit Data
•
Database Licensing
•
Web Design & Hosting
•
Trade Publications
Supplier List
•
Unit Converter
•
Reference
•
Links
•
Help
•
Contact Us
•
Site Map
•
FAQ
•
Home
Follow @MatWeb
Please read our
License Agreement
regarding materials data and our
Privacy Policy
. Questions or comments about MatWeb? Please contact us at
webmaster@matweb.com
. We appreciate your input.
The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.