MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Metalmen Sales

(Viewing data as-entered. Click here to return)
Titanium Ti-6Al-2Nb-1Ta-0.8Mo (Ti-621/0.8), Alpha-Annealed
Categories: Metal; Nonferrous Metal; Titanium Alloy; Alpha/Near Alpha Titanium Alloy

Material Notes: Alpha-annealed at 870ºC. Alpha Alloy.

High toughness, excellent weldability, resistance to corrosion in salt water.

Increasing oxygen impurity results in increasing beta transus and decreasing grain size.

Applications: Submersible hulls, pressure vessels

3 other heat treatments of this alloy are in MatWeb.

Key Words: Ti-621/0.8; UNS R56210; Ti-6211
Vendors: Visit metalmen for your metals needs. Products include special chemistry, tight tolerances, custom tempers, odd dimensions/forms, and small quantities. Phone 1-800-767-9494.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Density 4.48 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Brinell 290Estimated from Rockwell C.
Hardness, Knoop 315Estimated from Rockwell C.
Hardness, Rockwell C 30
Hardness, Vickers 304Estimated from Rockwell C.
Tensile Strength, Ultimate 830 MPa
Tensile Strength, Yield 710 MPa
Elongation at Break 11 %
Reduction of Area 30 %Average of Longitudinal and Transverse
Tensile Modulus 115 GPaValue for annealed sample
Compressive Yield Strength 790 MPa
Poissons Ratio 0.31
Fatigue Strength 170 MPa
@# of Cycles 1.00e+7
Kt (stress concentration factor) = 3.0
 280 MPa
@# of Cycles 1.00e+7
Unnotched
Fracture Toughness 99.0 MPa-m½KIC
Shear Modulus 43.9 GPaCalculated
Shear Strength 580 MPaUltimate shear strength
Charpy Impact 42.0 JV-notch
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.000160 ohm-cm
 
Thermal PropertiesOriginal ValueComments
CTE, linear 9.00 µm/m-°C
@Temperature 20.0 - 615 °C
average
 9.20 µm/m-°C
@Temperature 20.0 - 93.0 °C
Specific Heat Capacity 0.552 J/g-°C
Thermal Conductivity 6.40 W/m-K
Melting Point <= 1650 °C
Liquidus 1650 °C
Beta Transus 1110 °C
 
Component Elements PropertiesOriginal ValueComments
Aluminum, Al 6.0 %
Carbon, C <= 0.030 %
Hydrogen, H <= 0.10 %
Iron, Fe <= 0.12 %
Molybdenum, Mo 0.80 %
Niobium, Nb (Columbium, Cb) 2.0 %
Nitrogen, N <= 0.020 %
Other, each <= 0.10 %
Other, total <= 0.40 %
Oxygen, O <= 0.10 %
Tantalum, Ta 1.0 %
Titanium, Ti 90 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Titanium Ti-6Al-2Nb-1Ta-0.8Mo (Ti-621/0.8), STA-1
Titanium Ti-6Al-2Nb-1Ta-0.8Mo (Ti-621/0.8), STA
Titanium Ti-6Al-2Nb-1Ta-0.8Mo (Ti-621/0.8), as-rolled
Titanium Ti-6Al-2Sn-4Zr-2Mo-0.1Si; Duplex Annealed
Titanium Ti-6Al-2Nb-1Ta-1Mo, Annealed

MTA182 / 14118

Metalmen Sales

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.