MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

Ohara S-LAH95 Optical Glass
Categories: Ceramic; Glass; Optical

Material Notes:

Information provided by Ohara Corporation.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 4.64 g/cc4.64 g/cc
 
Chemical PropertiesMetricEnglishComments
Acid Class, SR 4.04.0
 
Mechanical PropertiesMetricEnglishComments
Hardness, Knoop 630
@Load 0.0999 kg
630
@Load 0.220 lb
Modulus of Elasticity 117.7 GPa17070 ksi
Modulus of Rigidity 45.2 GPa6560 ksi
Poissons Ratio 0.3020.302
Abrasion 8585Aa
 
Thermal PropertiesMetricEnglishComments
CTE, linear  7.30 µm/m-°C
@Temperature -30.0 - 70.0 °C
4.06 µin/in-°F
@Temperature -22.0 - 158 °F
 8.70 µm/m-°C
@Temperature 100 - 300 °C
4.83 µin/in-°F
@Temperature 212 - 572 °F
Thermal Conductivity 0.861 W/m-K
@Temperature 35.0 °C
5.98 BTU-in/hr-ft²-°F
@Temperature 95.0 °F
Transformation Temperature, Tg 649 °C1200 °Fper thermal expansion curve
Softening Point 713 °C1320 °F107.65 poise; JIS-R3104 and ASTM-C338
Annealing Point 638 °C1180 °F1013 poise; ASTM-C336
Strain Point 615 °C1140 °F1014.5 poise; JIS-R3103 and ASTM-C336
 
Optical PropertiesMetricEnglishComments
Refractive Index  1.84825
@Wavelength 2325.42 nm
1.84825
@Wavelength 2325.42 nm
 1.8553
@Wavelength 1970.09 nm
1.8553
@Wavelength 1970.09 nm
 1.86342
@Wavelength 1529.58 nm
1.86342
@Wavelength 1529.58 nm
 1.87194
@Wavelength 1128.64 nm
1.87194
@Wavelength 1128.64 nm
 1.87523
@Wavelength 1013.98 nm
1.87523
@Wavelength 1013.98 nm
nt (Hg t line)
 1.88155
@Wavelength 852.11 nm
1.88155
@Wavelength 852.11 nm
ns (Cs s line)
 1.88622
@Wavelength 768.19 nm
1.88622
@Wavelength 768.19 nm
nA' (K A' line)
 1.89068
@Wavelength 706.52 nm
1.89068
@Wavelength 706.52 nm
nr (He r line)
 1.89528
@Wavelength 656.27 nm
1.89528
@Wavelength 656.27 nm
nC (H C line)
 1.89659
@Wavelength 643.85 nm
1.89659
@Wavelength 643.85 nm
nC' (Cd C' line)
 1.89782
@Wavelength 632.8 nm
1.89782
@Wavelength 632.8 nm
nHe-Ne
 1.90341
@Wavelength 589.29 nm
1.90341
@Wavelength 589.29 nm
nD
 1.90366
@Wavelength 587.56 nm
1.90366
@Wavelength 587.56 nm
nd (He D line)
 1.91048
@Wavelength 546.07 nm
1.91048
@Wavelength 546.07 nm
ne (Hg e line)
 1.92411
@Wavelength 486.13 nm
1.92411
@Wavelength 486.13 nm
nf (H F line)
 1.92586
@Wavelength 479.99 nm
1.92586
@Wavelength 479.99 nm
nF' (Cd F' line)
 1.93896
@Wavelength 441.57 nm
1.93896
@Wavelength 441.57 nm
nHe-Cd
 1.9413
@Wavelength 435.835 nm
1.9413
@Wavelength 435.835 nm
ng (Hg g line)
 1.95648
@Wavelength 404.656 nm
1.95648
@Wavelength 404.656 nm
nh (Hg h line)
Abbe Number 31.131.1ν e
 31.3431.34ν d
Optical Dispersion 0.0083830.008383nd-nC; Partial Dispersion
 0.0090570.009057nC-nA'; Partial Dispersion
 0.013890.01389ne-nC'; Partial Dispersion
 0.0151780.015178nh-ng; Partial Dispersion
 0.0151990.015199ne-nC; Partial Dispersion
 0.0153820.015382nF'-ne; Partial Dispersion
 0.0171920.017192ng-nF; Partial Dispersion
 0.0200470.020047nC-nt; Partial Dispersion
 0.0213560.021356nC'-nt; Partial Dispersion
 0.0288320.028832nF-nC
 0.0292720.029272nF'-nC'
 0.0376410.037641ng-nd; Partial Dispersion
Transmission, Visible  56 %
@Thickness 10.0 mm,
Wavelength 380 nm
56 %
@Thickness 0.394 in,
Wavelength 380 nm
Internal Transmission
 71 %
@Thickness 10.0 mm,
Wavelength 390 nm
71 %
@Thickness 0.394 in,
Wavelength 390 nm
Internal Transmission
 80 %
@Thickness 10.0 mm,
Wavelength 400 nm
80 %
@Thickness 0.394 in,
Wavelength 400 nm
Internal Transmission
 89 %
@Thickness 10.0 mm,
Wavelength 420 nm
89 %
@Thickness 0.394 in,
Wavelength 420 nm
Internal Transmission
 93.4 %
@Thickness 10.0 mm,
Wavelength 440 nm
93.4 %
@Thickness 0.394 in,
Wavelength 440 nm
Internal Transmission
 95.6 %
@Thickness 10.0 mm,
Wavelength 460 nm
95.6 %
@Thickness 0.394 in,
Wavelength 460 nm
Internal Transmission
 97 %
@Thickness 10.0 mm,
Wavelength 480 nm
97 %
@Thickness 0.394 in,
Wavelength 480 nm
Internal Transmission
 98 %
@Thickness 10.0 mm,
Wavelength 500 nm
98 %
@Thickness 0.394 in,
Wavelength 500 nm
Internal Transmission
 99.2 %
@Thickness 10.0 mm,
Wavelength 550 nm
99.2 %
@Thickness 0.394 in,
Wavelength 550 nm
Internal Transmission
 99.5 %
@Thickness 10.0 mm,
Wavelength 600 nm
99.5 %
@Thickness 0.394 in,
Wavelength 600 nm
Internal Transmission
 99.6 %
@Thickness 10.0 mm,
Wavelength 650 nm
99.6 %
@Thickness 0.394 in,
Wavelength 650 nm
Internal Transmission
 99.7 %
@Thickness 10.0 mm,
Wavelength 700 nm
99.7 %
@Thickness 0.394 in,
Wavelength 700 nm
Internal Transmission
IR Transmittance  81 %
@Thickness 10.0 mm,
Wavelength 2400 nm
81 %
@Thickness 0.394 in,
Wavelength 2400 nm
Internal Transmission
 93.3 %
@Thickness 10.0 mm,
Wavelength 2200 nm
93.3 %
@Thickness 0.394 in,
Wavelength 2200 nm
Internal Transmission
 97.2 %
@Thickness 10.0 mm,
Wavelength 2000 nm
97.2 %
@Thickness 0.394 in,
Wavelength 2000 nm
Internal Transmission
 98.8 %
@Thickness 10.0 mm,
Wavelength 1800 nm
98.8 %
@Thickness 0.394 in,
Wavelength 1800 nm
Internal Transmission
 99.5 %
@Thickness 10.0 mm,
Wavelength 1600 nm
99.5 %
@Thickness 0.394 in,
Wavelength 1600 nm
Internal Transmission
 99.7 %
@Thickness 10.0 mm,
Wavelength 1400 nm
99.7 %
@Thickness 0.394 in,
Wavelength 1400 nm
Internal Transmission
 99.8 %
@Thickness 10.0 mm,
Wavelength 800 nm
99.8 %
@Thickness 0.394 in,
Wavelength 800 nm
Internal Transmission
 99.8 %
@Thickness 10.0 mm,
Wavelength 900 nm
99.8 %
@Thickness 0.394 in,
Wavelength 900 nm
Internal Transmission
 99.8 %
@Thickness 10.0 mm,
Wavelength 1000 nm
99.8 %
@Thickness 0.394 in,
Wavelength 1000 nm
Internal Transmission
 99.9 %
@Thickness 10.0 mm,
Wavelength 1200 nm
99.9 %
@Thickness 0.394 in,
Wavelength 1200 nm
Internal Transmission
UV Transmittance  6.0 %
@Thickness 10.0 mm,
Wavelength 360 nm
6.0 %
@Thickness 0.394 in,
Wavelength 360 nm
Internal Transmission
 31 %
@Thickness 10.0 mm,
Wavelength 370 nm
31 %
@Thickness 0.394 in,
Wavelength 370 nm
Internal Transmission
 
Descriptive Properties
Acid Resistance, Powder Method, RA(P)1
CCI0.00 B
 4.11 G
 4.11 R
coloring, λ 5360
coloring, λ 70410
Coloring, Internal Transmission λ 0.05360
Coloring, Internal Transmission λ 0.80400
Knoop Hardness Class6
Ohara Code d904313
Ohara Code e910311
Phosphate Resistance, PR1
Photoelastic Constant (ß)1.43
Water Resistance, RW(P)1
Weathering Resistance (Surface Method) W(S)max1
Yield Point, At (°C)684per thermal expansion curve

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

CZOHARA767 / 281606

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.