MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

Sandvik SANMAC 316/316L Billet
Categories: Metal; Ferrous Metal; Alloy Steel; Austenitic

Material Notes: Sanmac 316/316L, 1.4401/1.4404, is a molybdenum-alloyed austenitic chromium-nickel steel with improved machinability.

Information provided by Sandvik

ASTM 316, 316L; UNS S31603, S31600; EN 1.4404, 1.4401

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 7.90 g/cc0.285 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Brinell 170170
Tensile Strength, Ultimate 515 - 690 MPa74700 - 100000 psi
 >= 360 MPa
@Temperature 500 °C
>= 52200 psi
@Temperature 932 °F
 >= 380 MPa
@Temperature 300 °C
>= 55100 psi
@Temperature 572 °F
 >= 380 MPa
@Temperature 400 °C
>= 55100 psi
@Temperature 752 °F
 >= 400 MPa
@Temperature 200 °C
>= 58000 psi
@Temperature 392 °F
 >= 450 MPa
@Temperature 100 °C
>= 65300 psi
@Temperature 212 °F
Tensile Strength, Yield  >= 205 MPa
@Strain 0.2 %
>= 29700 psi
@Strain 0.2 %
 >= 240 MPa
@Strain 1 %
>= 34800 psi
@Strain 1 %
 >= 92.0 MPa
@Strain 0.2 %,
Temperature 500 °C
>= 13300 psi
@Strain 0.2 %,
Temperature 932 °F
 >= 98.0 MPa
@Strain 0.2 %,
Temperature 400 °C
>= 14200 psi
@Strain 0.2 %,
Temperature 752 °F
 >= 110 MPa
@Strain 0.2 %,
Temperature 300 °C
>= 16000 psi
@Strain 0.2 %,
Temperature 572 °F
 >= 120 MPa
@Strain 1 %,
Temperature 500 °C
>= 17400 psi
@Strain 1 %,
Temperature 932 °F
 >= 125 MPa
@Strain 1 %,
Temperature 400 °C
>= 18100 psi
@Strain 1 %,
Temperature 752 °F
 >= 127 MPa
@Strain 0.2 %,
Temperature 200 °C
>= 18400 psi
@Strain 0.2 %,
Temperature 392 °F
 >= 135 MPa
@Strain 1 %,
Temperature 300 °C
>= 19600 psi
@Strain 1 %,
Temperature 572 °F
 >= 155 MPa
@Strain 0.2 %,
Temperature 100 °C
>= 22500 psi
@Strain 0.2 %,
Temperature 212 °F
 >= 155 MPa
@Strain 1 %,
Temperature 200 °C
>= 22500 psi
@Strain 1 %,
Temperature 392 °F
 >= 190 MPa
@Strain 1 %,
Temperature 100 °C
>= 27600 psi
@Strain 1 %,
Temperature 212 °F
Elongation at Break >= 40 %>= 40 %
Reduction of Area >= 50 %>= 50 %
Modulus of Elasticity 200 GPa29000 ksi
 165 GPa
@Temperature 500 °C
23900 ksi
@Temperature 932 °F
 172 GPa
@Temperature 400 °C
24900 ksi
@Temperature 752 °F
 179 GPa
@Temperature 300 °C
26000 ksi
@Temperature 572 °F
 186 GPa
@Temperature 200 °C
27000 ksi
@Temperature 392 °F
 194 GPa
@Temperature 100 °C
28100 ksi
@Temperature 212 °F
Charpy Impact >= 100 J>= 73.8 ft-lb
 
Thermal PropertiesMetricEnglishComments
CTE, linear  16.5 µm/m-°C
@Temperature 30.0 - 100 °C
9.17 µin/in-°F
@Temperature 86.0 - 212 °F
 17.0 µm/m-°C
@Temperature 30.0 - 200 °C
9.44 µin/in-°F
@Temperature 86.0 - 392 °F
 17.5 µm/m-°C
@Temperature 30.0 - 300 °C
9.72 µin/in-°F
@Temperature 86.0 - 572 °F
 18.0 µm/m-°C
@Temperature 30.0 - 500 °C
10.0 µin/in-°F
@Temperature 86.0 - 932 °F
 18.0 µm/m-°C
@Temperature 30.0 - 400 °C
10.0 µin/in-°F
@Temperature 86.0 - 752 °F
 18.5 µm/m-°C
@Temperature 30.0 - 600 °C
10.3 µin/in-°F
@Temperature 86.0 - 1110 °F
 18.5 µm/m-°C
@Temperature 30.0 - 700 °C
10.3 µin/in-°F
@Temperature 86.0 - 1290 °F
Specific Heat Capacity  0.485 J/g-°C
@Temperature 20.0 °C
0.116 BTU/lb-°F
@Temperature 68.0 °F
 0.500 J/g-°C
@Temperature 100 °C
0.120 BTU/lb-°F
@Temperature 212 °F
 0.515 J/g-°C
@Temperature 200 °C
0.123 BTU/lb-°F
@Temperature 392 °F
 0.525 J/g-°C
@Temperature 300 °C
0.125 BTU/lb-°F
@Temperature 572 °F
 0.540 J/g-°C
@Temperature 400 °C
0.129 BTU/lb-°F
@Temperature 752 °F
 0.555 J/g-°C
@Temperature 500 °C
0.133 BTU/lb-°F
@Temperature 932 °F
 0.575 J/g-°C
@Temperature 600 °C
0.137 BTU/lb-°F
@Temperature 1110 °F
Thermal Conductivity  14.0 W/m-K
@Temperature 20.0 °C
97.2 BTU-in/hr-ft²-°F
@Temperature 68.0 °F
 15.0 W/m-K
@Temperature 100 °C
104 BTU-in/hr-ft²-°F
@Temperature 212 °F
 17.0 W/m-K
@Temperature 200 °C
118 BTU-in/hr-ft²-°F
@Temperature 392 °F
 18.0 W/m-K
@Temperature 300 °C
125 BTU-in/hr-ft²-°F
@Temperature 572 °F
 20.0 W/m-K
@Temperature 400 °C
139 BTU-in/hr-ft²-°F
@Temperature 752 °F
 21.0 W/m-K
@Temperature 500 °C
146 BTU-in/hr-ft²-°F
@Temperature 932 °F
 23.0 W/m-K
@Temperature 600 °C
160 BTU-in/hr-ft²-°F
@Temperature 1110 °F
 
Component Elements PropertiesMetricEnglishComments
Carbon, C <= 0.030 %<= 0.030 %
Chromium, Cr 16.5 %16.5 %
Iron, Fe 67.9 %67.9 %As Balance
Manganese, Mn 1.8 %1.8 %
Molybdenum, Mo 2.1 %2.1 %
Nickel, Ni 11 %11 %
Phosphorus, P <= 0.040 %<= 0.040 %
Silicon, Si 0.60 %0.60 %
Sulfur, S <= 0.030 %<= 0.030 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
AISI Type 316L Stainless Steel, annealed sheet
Outokumpu 4404 Cr-Ni-Mo Austenitic Stainless Steel
316 Stainless Steel, annealed bar
AISI Type 316L Stainless Steel, annealed plate
AISI Type 316L Stainless Steel, annealed strip

NSANDV182 / 19076

Free Trade Publications, Click Here!
Free Trade Publications, Click Here!

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.