MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

Elektro-Isola Etronax MF G Phenolic, Cotton Fabric Reinforcement, Black, Sheets
Categories: Polymer; Thermoset; Phenolic

Material Notes: Description: Exclusively for mechanical applications. Impact-resistant. Resistant to mechanical wear and noise-reducing. The graphite content causes low friction. Well suited for parts where there are high mechanical load and wear requirements. Good wear resistance in aggressive and dust-filled environments. Can be lubricated with water, oil or grease. Alternative to materials containing asbestos.

Information provided by Elektro-Isola

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.40 g/cc
@Temperature 23.0 °C
0.0506 lb/in³
@Temperature 73.4 °F
24h/23°C/50% RH; ISO 1183-A
Water Absorption 1.1 %1.1 %ISO 62-1
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength 80.0 MPa
@Thickness >=1.50 mm
11600 psi
@Thickness >=0.0591 in
24h/23°C/50% RH; ISO 527
Flexural Strength 135 MPa
@Thickness >=1.50 mm
19600 psi
@Thickness >=0.0591 in
24h/23°C/50% RH, Normal to laminate plane; ISO 178
Flexural Modulus 7.00 GPa
@Thickness >=1.50 mm
1020 ksi
@Thickness >=0.0591 in
24h/23°C/50% RH, Normal to laminate plane; ISO 178
Compressive Strength 330 MPa
@Thickness >=5.00 mm
47900 psi
@Thickness >=0.197 in
24h/23°C/50% RH, , Normal to laminate plane; ISO 604
Shear Strength 50.0 MPa
@Thickness >=5.00 mm
7250 psi
@Thickness >=0.197 in
Parallel, 24h/23°C/50% RH; IEC 60893-2
Izod Impact, Notched (ISO) 10.0 kJ/m²
@Thickness >=5.00 mm
4.76 ft-lb/in²
@Thickness >=0.197 in
Parallel, 24h/23°C/50% RH; ISO 180/2A
 
Thermal PropertiesMetricEnglishComments
Maximum Service Temperature, Air 100 °C
@Thickness >=3.00 mm,
Time 7.20e+7 sec
212 °F
@Thickness >=0.118 in,
Time 20000 hour
IEC 60216
 
Descriptive Properties
ColorBlack

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
3M Safety-Walk™ 5100 Cushion Matting

PELEKT040 / 126916

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.