MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
Uninhibited Leaded Muntz Metal, UNS C36500
Categories: Metal; Nonferrous Metal; Copper Alloy

Material Notes: Fair to excellent corrosion resistance. Excellent machinability. Combines good machinability with excellent hot formability.

Applications: main tube sheets for condensers and heat exchangers, support sheets, baffles.

Commercial forms available flat products. Rod 61.0% Cu minimum.

Key Words: 60/40 brass, CDA 365, CZ137, ISO, CuZn39Pb0.5, CEN CW610N, uninhibited, arsenical, antimonial, phosphorized leaded muntz metal, low leaded brass
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 8.41 g/ccUNS C36500
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell F 80M20 temper
Tensile Strength, Ultimate 370 MPaM20 temper
Tensile Strength, Yield 140 MPaM20 temper
Elongation at Break 45 %in 50 mm, M20 temper
Modulus of Elasticity 105 GPa
Poissons Ratio 0.35Calculated
Machinability 60 %UNS C36000 (free-cutting brass) = 100%
Shear Modulus 39.0 GPa
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.00000620 ohm-cm
@Temperature 20.0 °C
 
Thermal PropertiesOriginal ValueComments
CTE, linear 20.8 µm/m-°C
@Temperature 20.0 - 300 °C
Specific Heat Capacity 0.380 J/g-°C
Thermal Conductivity 123 W/m-K
@Temperature 20.0 °C
Melting Point 885 - 900 °C
Solidus 885 °C
Liquidus 900 °C
 
Processing PropertiesOriginal ValueComments
Annealing Temperature 425 - 600 °C
Hot-Working Temperature 625 - 800 °C
 
Component Elements PropertiesOriginal ValueComments
Copper, Cu 58 - 61 %
Iron, Fe <= 0.15 %
Lead, Pb 0.40 - 0.90 %
Other, total <= 0.10 %
Tin, Sn <= 0.25 %
Zinc, Zn 39.4 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Arsenical Leaded Muntz Metal, UNS C36600
Architectural Bronze, UNS C38500
Forging Brass, UNS C37700
Arsenical Naval brass, UNS C46500, O61 Temper tubing
Phosphorized Naval brass, UNS C46700, O61 Temper tubing

MC36500b1 / 11245

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.