MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
LyondellBasell Hostalen PP H4122 103220 Polypropylene Copolymer
Categories: Polymer; Thermoplastic; Polypropylene (PP); Polypropylene Copolymer

Material Notes: Hostalen PP H4122 103220 is a black colored polypropylene block copolymer. The product is typically used in the application of pipe extrusion. The material Hostalen PP H4122 103220 is not intended for medical and pharmaceutical applications. Applications: Industrial, Plumbing, Heating & Cooling

Information provided by LyondellBasell.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 0.908 g/ccISO 1183-1
Melt Flow 0.30 g/10 min
@Load 2.16 kg,
Temperature 230 °C
ISO 1133-1
 0.50 g/10 min
@Load 5.00 kg,
Temperature 190 °C
ISO 1133-1
 1.3 g/10 min
@Load 5.00 kg,
Temperature 230 °C
ISO 1133-1
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore D 60ISO 868
Ball Indentation Hardness 50.0 MPaISO 2039-1
Tensile Strength, Yield 30.0 MPaISO 527-1,-2
Elongation at Yield 13 %ISO 527-1,-2
Tensile Modulus 1400 MPaISO 527-1,-2
Charpy Impact, Notched 5.80 kJ/m²
@Temperature -30.0 °C
ISO 179
 20.0 kJ/m²
@Temperature 0.000 °C
ISO 179
 110 kJ/m²
@Temperature 23.0 °C
ISO 179
 
Thermal PropertiesOriginal ValueComments
Vicat Softening Point 83.0 °CB50; ISO 306
 159 °CA50; ISO 306
 
Descriptive Properties
Processing Methodinjection molding, pipe

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
LyondellBasell Hostalen PP H5416 Polypropylene Copolymer
Inno-Comp INNOPOL® CS 3-8000 FR Flame Retardant Polypropylene Blend
Borealis RA130E-8427 Polypropylene Random Copolymer
Ascend Performance Materials Starflam® M10009AP PP, Flame Retardant, Injection Molding
LyondellBasell Hostalen PP HP1886 Polypropylene Copolymer

PEQT8516 / 220151

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.