MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
Hexcel® HexBond™ EA9321 STRUCTIL Epoxy Paste Adhesive
Categories: Polymer; Thermoset; Epoxy; Epoxy Adhesive

Material Notes: Description: Thixotropic two-part epoxy adhesive. Its viscosity allows to be used for potting, edge filling, shimming, fairing and bonding applications.

Features:

  • Room temperature cure (= 18°C/64°F)
  • Outstanding mechanical properties over a wide range of temperatures (-55°C/-67°F to 120°C/250°F)

Information provided by Hexcel Corporation.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.24 g/ccPart B
 1.25 g/ccMixture
 1.31 g/ccPart A
Brookfield Viscosity 35000 - 100000 cPPart B
 300000 - 600000 cPPart A
 1.60e+6 cPMixed
 
Mechanical PropertiesOriginal ValueComments
Adhesive Bond Strength 4.50 MPa
@Temperature 180 °C
Lap Shear; EN 2243-1
 9.00 MPa
@Temperature 120 °C
Lap Shear; EN 2243-1
 14.0 MPa
@Temperature 100 °C
Lap Shear; EN 2243-1
 15.0 MPa
@Temperature 80.0 °C
Lap Shear; EN 2243-1
 22.5 MPa
@Temperature 22.8 °C
Lap Shear, Wet ageing 70°C/158°F, 85% RH (saturation); EN 2243-1
 24.0 MPa
@Temperature -55.0 °C
Lap Shear; EN 2243-1
 27.0 MPa
@Temperature 22.8 °C
Lap Shear; EN 2243-1
Peel Strength 3.00 kN/mBell, 23°C
 
Processing PropertiesOriginal ValueComments
Shelf Life 3.00 Month
@Temperature 25.0 °C
Part B
 12.0 Month
@Temperature 4.00 °C
Part A
 12.0 Month
@Temperature 4.00 °C
Part A
 12.0 Month
@Temperature 25.0 °C
Part B
 
Descriptive Properties
ColorGreyMixture
 GreyPart A
 Off-whitePart B

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PHEXCB9285 / 322441

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.