MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

United Soft Plastics Unisoft Polaric AK-65A-CL-1-01 Acrylic-based Thermoplastic Elastomer (TPE-A)
Categories: Polymer; Thermoplastic; Elastomer, TPE

Material Notes: This compound has superior oil resistance, high clarity, and excellent adhesion to a variety of substrates. It is available worldwide.

Features:

  • Easily Colorable
  • Heat Stabilized
  • Oil & Fat Resistant
  • Excellent Chemical Resistance
  • High Clarity

Information provided by United Soft Plastics.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.09 g/cc0.0394 lb/in³
Linear Mold Shrinkage 0.014 - 0.023 cm/cm0.014 - 0.023 in/in
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A 6565
Tensile Strength 12.24 MPa1775 psi
Elongation at Break 340 %340 %
100% Modulus 4.79 MPa
@Strain 100 %
695 psi
@Strain 100 %
 
Processing PropertiesMetricEnglishComments
Rear Barrel Temperature 160 - 174 °C320 - 345 °F
Middle Barrel Temperature 171 - 196 °C340 - 385 °F
Front Barrel Temperature 179 - 204 °C355 - 400 °F
Nozzle Temperature 179 - 204 °C355 - 400 °F
Drying Temperature 71.1 °C
@Time 5400 - 7200 sec
160 °F
@Time 1.50 - 2.00 hour
 
Descriptive Properties
BondingPMMA, PA-6, PC, PET, ABS, PS, PVC, TPU
ColorsWater Clear
ProcessingInjection Molding & Extrusion
Relative FlowMedium

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PUSOF9844 / 243347

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.