MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Taro Plast Taroblend B35 G2 ABS/PA, 8% Glass Fiber Reinforced
Categories: Polymer; Thermoplastic; ABS Polymer; Acrylonitrile Butadiene Styrene (ABS)/Nylon Blend, Glass Reinforced

Material Notes: ABS/PA alloy, 8% glass fibers reinforced, combining good impact strength with chemical resistance, designed according to European dir. 2000/53/EC (End-of-Life Vehicle). Available: all colors, UV stabilized (L).

Information provided by Taro Plast S.p.a.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.12 g/ccISO 1183
Filler Content 8.0 %ISO 3451
Water Absorption at Saturation 1.4 %ISO 62
Linear Mold Shrinkage, Flow 0.0050 cm/cmISO 2577
Linear Mold Shrinkage, Transverse 0.0080 cm/cmISO 2577
Melt Flow 30 g/10 min
@Load 10.0 kg,
Temperature 240 °C
ISO 1133
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength at Break 54.0 MPaISO 527
Elongation at Break 6.0 %ISO 527
Tensile Modulus 3100 MPaISO 527
Flexural Strength 74.0 MPaISO 178
Flexural Modulus 2850 MPaISO 178
Izod Impact, Notched 60.0 J/m
@Temperature -20.0 °C
127x12.7x3.2; ASTM D256
 720 J/m
@Temperature 23.0 °C
127x12.7x3.2; ASTM D256
Charpy Impact, Notched 11.0 kJ/m²80x10x4; ISO 179/1eA
 
Electrical PropertiesOriginal ValueComments
Comparative Tracking Index >= 600 VMethod A; IEC 60112
 
Thermal PropertiesOriginal ValueComments
CTE, linear 60.0 µm/m-°CISO 11359
Deflection Temperature at 0.46 MPa (66 psi) 135 °CISO 75/A
Deflection Temperature at 1.8 MPa (264 psi) 85.0 °CISO 75/A
Vicat Softening Point 115 °C
@Load 5.00 kg
ISO 306
 180 °C
@Load 1.00 kg
ISO 306
Flammability, UL94 HB
@Thickness 1.60 mm
127x2.17xThickness
Glow Wire Flammability Index 650 °C
@Thickness 2.00 mm
60x60xThickness; IEC 60695-2-12

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PTARO116 / 283224

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.