MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Specialty Compounds RTP Company

Solvay LTM® 123 Cyanate Ester Prepreg with CF0300 Carbon Fabric
Categories: Polymer; Thermoset; Carbon Fiber/Thermoset Composite; Polyester, TS

Material Notes: LTM123 is a low temperature curing, toughened cyanate ester component prepreg developed for structural applications requiring ultimate dimensional stability in a space environment. Its low moisture absorption and low electrical permittivity characteristics also make it suitable for radomes and radar absorbing structures. LTM123 is also suitable for high service temperature structural applications in the motorsport market. LTM123 can be processed using autoclave and oven vacuum bag methods to produce low voidage composites and can be molded off a range of low cost tooling with few constraints on structure dimensions. For space applications, LTM123 can develop a Tg of 140LC (248°F) after a minimum initial cure at 80°C (176°F) and a free-standing post-cure of 120°C (248°F). For motorsport applications, LTM123 can develop a Tg of 250°C (482°F) after a minimum initial cure at 80°C (176°F) and free-standing post-cure of 240°C (464°F).

Features & Benefits:

  • 3 days tack life at 21°C (70°F)
  • 6 months storage at -18°C (0°F)
  • 70°C (158°F) initial cure
  • Autoclave cure
  • Good dimensional stability and thermal durability up to 250°C (482°f) after post-cure
  • Maximum Tg of 330°C (626°F); can withstand thermal spikes to 330°C (626°F)
  • Inherently flame retardant, with low toxic gas and smoke generation
  • Good dielectric properties for radar transparency
Property data reported for dry conditions: LTM123/CF0300 2x2 twill, 199 g/m2 fabric with 3k HS fibers; Cure: 16 hrs at 80°C (176°F), 6.2 bar (90 psi); Post-cure: 3 hrs at 200°C (392°F). Compressive and tensile properties normalized to 55 vol%.

Information provided by Cytec, subsequently acquired by Solvay.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Moisture Absorption at Equilibrium 0.22 %0.22 %0 to 60% RH, 60°C, (1.5mm 0°±60°C M55J reinforcement)
Storage Temperature -18.0 °C-0.400 °FLTM® 123
 
Mechanical PropertiesMetricEnglishComments
Flexural Strength  899.1 MPa
@Temperature 177 °C
130400 psi
@Temperature 351 °F
0/90°; CRAG 200
 994.9 MPa
@Temperature 24.0 °C
144300 psi
@Temperature 75.2 °F
0/90°; CRAG 200
Flexural Modulus  56.0 GPa
@Temperature 24.0 °C
8120 ksi
@Temperature 75.2 °F
0/90°; CRAG 200
 57.0 GPa
@Temperature 177 °C
8270 ksi
@Temperature 351 °F
0/90°; CRAG 200
Compressive Strength 143 MPa20700 psiQuasi-Isotropic after 6.7 J/mm Impact; SACMA SRM 2R-94
 533 MPa
@Temperature 177 °C
77300 psi
@Temperature 351 °F
0/90°; ASTM D3410
Shear Strength  46.9 MPa
@Temperature 177 °C
6800 psi
@Temperature 351 °F
0/90° Interlaminar; ASTM D2344
 75.2 MPa
@Temperature 24.0 °C
10900 psi
@Temperature 75.2 °F
0/90° Interlaminar; ASTM D2344
 
Thermal PropertiesMetricEnglishComments
CTE, linear -1.02 - -0.980 µm/m-°C
@Temperature 20.0 - 80.0 °C
-0.567 - -0.544 µin/in-°F
@Temperature 68.0 - 176 °F
0°; M55J reinforcement
 
Processing PropertiesMetricEnglishComments
Cure Time 180 min
@Temperature 200 °C
3.00 hour
@Temperature 392 °F
Post-cure As Tested
 960 min
@Pressure 0.621 MPa,
Temperature 80.0 °C
16.0 hour
@Pressure 90.0 psi,
Temperature 176 °F
As Tested
Shelf Life 6.00 Month
@Temperature -18.0 °C
6.00 Month
@Temperature -0.400 °F
LTM® 123

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PCYTED178f / 240087

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.