Envalior Durethan® BKV 215 W1 902176 Nylon 6 (PA6), 15% Glass Fiber Reinforced, Dry
Categories:
Polymer
;
Thermoplastic
;
Nylon (Polyamide PA)
;
Nylon 6 (PA6)
;
Nylon 6, 20% Glass Fiber Filled
Material Notes:
PA 6-Copolymer, 15% glass fibers, injection molding, improved impact strength, weather stabilized
Former Lanxess product line is now with Envalior.
Vendors:
No vendors are listed for this material. Please
click here
if you are a supplier and would like information on how to add your listing to this material.
Printer friendly version
Download as PDF
Download to Excel (requires Excel and Windows)
Export data to your CAD/FEA program
Add to Folder:
My Folder
Physical Properties
Metric
English
Comments
Density
1.18
g/cc
0.0426
lb/in³
ISO 1183
Linear Mold Shrinkage, Flow
0.0050
cm/cm
0.0050
in/in
60x60x2; 280 °C / MT 80°C; 600 bar; ISO 294-4
Linear Mold Shrinkage, Transverse
0.0060
cm/cm
0.0060
in/in
60x60x2; 280 °C / MT 80°C; 600 bar; ISO 294-4
Mechanical Properties
Metric
English
Comments
Puncture Resistance
785
N
@Temperature -30.0 °C
176
lb (f)
@Temperature -22.0 °F
ISO 6603-2
1760
N
@Temperature 23.0 °C
396
lb (f)
@Temperature 73.4 °F
ISO 6603-2
Tensile Strength at Break
85.0
MPa
12300
psi
5 mm/min; ISO 527-1,-2
Elongation at Break
4.7 %
4.7 %
5 mm/min; ISO 527-1,-2
Tensile Modulus
4.40
GPa
638
ksi
1 mm/min; ISO 527-1,-2
Flexural Strength
135
MPa
19600
psi
2 mm/min; ISO 178-A
Flexural Yield Strength
115
MPa
@Strain 3.5 %
16700
psi
@Strain 3.5 %
2 mm/min; ISO 178-A
Flexural Modulus
3.90
GPa
566
ksi
2 mm/min; ISO 178-A
Flexural Strain at Break
5.5 %
5.5 %
2 mm/min; ISO 178-A
Izod Impact, Notched (ISO)
20.0
kJ/m²
@Temperature 23.0 °C
9.52
ft-lb/in²
@Temperature 73.4 °F
ISO 180-1A
Izod Impact, Unnotched (ISO)
55.0
kJ/m²
@Temperature 23.0 °C
26.2
ft-lb/in²
@Temperature 73.4 °F
ISO 180-1U
60.0
kJ/m²
@Temperature -30.0 °C
28.6
ft-lb/in²
@Temperature -22.0 °F
ISO 180-1U
Charpy Impact Unnotched
6.50
J/cm²
@Temperature 23.0 °C
30.9
ft-lb/in²
@Temperature 73.4 °F
ISO 179-1eU
8.00
J/cm²
@Temperature -30.0 °C
38.1
ft-lb/in²
@Temperature -22.0 °F
ISO 179-1eU
Puncture Energy
3.10
J
@Temperature -30.0 °C
2.29
ft-lb
@Temperature -22.0 °F
ISO 6603-2
7.30
J
@Temperature 23.0 °C
5.38
ft-lb
@Temperature 73.4 °F
ISO 6603-2
Electrical Properties
Metric
English
Comments
Comparative Tracking Index
600
V
600
V
Solution A; IEC 60112
Thermal Properties
Metric
English
Comments
CTE, linear, Parallel to Flow
50.0
µm/m-°C
@Temperature 23.0 - 55.0 °C
27.8
µin/in-°F
@Temperature 73.4 - 131 °F
ISO 11359-1,-2
CTE, linear, Transverse to Flow
160
µm/m-°C
@Temperature 23.0 - 55.0 °C
88.9
µin/in-°F
@Temperature 73.4 - 131 °F
ISO 11359-1,-2
Melting Point
214
°C
417
°F
10°C/min; ISO 11357-1,-3
Deflection Temperature at 0.46 MPa (66 psi)
205
°C
401
°F
ISO 75-1,-2
Deflection Temperature at 1.8 MPa (264 psi)
180
°C
356
°F
ISO 75-1,-2
Deflection Temperature at 8.0 MPa
60.0
°C
140
°F
ISO 75-1,-2
Vicat Softening Point
193
°C
@Load 5.10 kg
379
°F
@Load 11.2 lb
120°C/h; ISO 306
Shrinkage, MD
0.10 %
@Treatment Temp. 120 °C,
Time 14400 sec
0.10 %
@Treatment Temp. 248 °F,
Time 4.00 hour
Post-Shrinkage Flow Direction; 60x60x2; ISO 294-4
Shrinkage, TD
0.10 %
@Treatment Temp. 120 °C,
Time 14400 sec
0.10 %
@Treatment Temp. 248 °F,
Time 4.00 hour
60x60x2; ISO 294-4
Processing Properties
Metric
English
Comments
Melt Temperature
260
-
290
°C
500
-
554
°F
280
°C
536
°F
injection molding
Mold Temperature
80.0
°C
176
°F
injection molding
80.0
-
100
°C
176
-
212
°F
Drying Temperature
80.0
°C
176
°F
Dry Time
2.00
-
6.00
hour
2.00
-
6.00
hour
Moisture Content
0.030 - 0.12 %
0.030 - 0.12 %
Karl Fischer
Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's
terms of use
regarding this information.
Click here
to view all the property values for this datasheet as they were originally entered into MatWeb.
Users viewing this material also viewed the following:
Envalior Durethan® BKV 215 W1 902176 Nylon 6 (PA6), 15% Glass Fiber Reinforced, Conditioned
LyondellBasell Hostacom TYC727N NATRL Thermoplastic Olefinic Elastomer
LyondellBasell Hostacom M2 U02 C1 BLACK Polypropylene with 20% Talc Filler
Envalior Durethan® BKV 215 H2.0 DUS008 901510 Nylon 6, Impact Modified
PLANW9358 / 208177
Subscribe to Premium Services
Searches:
Advanced
•
Composition
•
Property
•
Material Type
•
Manufacturer
•
Trade Name
•
UNS Number
Other Links:
Advertising
•
Submit Data
•
Database Licensing
•
Web Design & Hosting
•
Trade Publications
Supplier List
•
Unit Converter
•
Reference
•
Links
•
Help
•
Contact Us
•
Site Map
•
FAQ
•
Home
Follow @MatWeb
Please read our
License Agreement
regarding materials data and our
Privacy Policy
. Questions or comments about MatWeb? Please contact us at
webmaster@matweb.com
. We appreciate your input.
The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.