MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

CRP  Windform

(Viewing data as-entered. Click here to return)
DSM Somos® 9420 Epoxy Resin for Stereolithography
Categories: Polymer; 3D Printing/Additive Manufacturing Polymer; Thermoset; Epoxy

Material Notes: Description

Somos® 9420 is an opaque white stereolithography resin that is easy to use and fast to process. This stereolithography resin produces accurate parts that are semiflexible. Parts produced with Somos® 9420 are comparable to polypropylene in mechanical properties and offer a good combination of flexibility and toughness. Somos® 9420 is ideal for applications such as the design and testing of snap-fits, electronic and automobile components as well as packaging.

Key Benefits:

  • Flexible
  • Incredible Memory Retention
  • Tough & Durable
  • Bright Opaque-White Color
Ideal Applications:
  • Prototypes where polypropylene will be the final production plastic
  • Packaging design
  • Snap fits, bottle tops, fittings

Information Provided by DSM Desotech Inc.

Vendors:
Proto3000 provides design tools, 3D printers, additive manufacturing processes, metrology technologies, high-performance materials, and part-finishing automation. Our ISO 9001:2015 additive manufacturing production facility offers 3D printing services, rapid prototyping services, and end-part production with HP MultiJet Fusion (MJF), FDM, SLA, SLS, Polyjet, DLP, metal binder jetting, BMD, and DMLS.


Axis Proto Inc. North American leaders for providing high quality Rapid Prototyping and Rapid Manufacturing solutions using all major Additive systems including Stereolithography printing. Free 3D printing quotes at www.axisproto.com

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Density 1.13 g/cc
@Temperature 25.0 °C
Water Absorption 0.93 %ASTM D570-98
Viscosity 475 cP
@Temperature 30.0 °C
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore D 72ASTM D2240
Elongation at Break 28 %ASTM D638M
Modulus of Elasticity 0.700 GPaASTM D638M
Flexural Strength 27.0 MPaASTM D790M
Flexural Modulus 834 MPaASTM D790M
Poissons Ratio 0.43ASTM D638M
Izod Impact, Notched 46.0 J/cmASTM D256A
 
Electrical PropertiesOriginal ValueComments
Dielectric Constant 3.94
@Frequency 1e+6 Hz
ASTM D150-98
 4.66
@Frequency 1000 Hz
ASTM D150-98
 5.33
@Frequency 60.0 Hz
ASTM D150-98
Dielectric Strength 14.1 kV/mmASTM D149-97a
 
Thermal PropertiesOriginal ValueComments
CTE, linear 96.8 µm/m-°C
@Temperature -40.0 - 0.000 °C
ASTM E831-00
 144 µm/m-°C
@Temperature 100 - 150 °C
ASTM E831-00
 149.5 µm/m-°C
@Temperature 0.000 - 50.0 °C
ASTM E831-00
 178.7 µm/m-°C
@Temperature 50.0 - 100 °C
ASTM E831-00
Deflection Temperature at 0.46 MPa (66 psi) 49.0 °CASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 37.0 °CASTM D648
 
Descriptive Properties
AppearanceWhite
Dp (mm)0.14Slope of cure-depth vs. ln(E) curve
E10 (mJ/cm2)95Exposure that gives 0.254mm thickness
Ec (mJ/cm2)15Critical exposure

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
DSM Somos® NanoTool™ Resin for Stereolithography, UV Postcure
3D Systems Accura® ClearVue™ Free (SL 7870) Stereolithography Plastic
DSM Somos® 14120 Water-resistant resin for stereolithography, White
3D Systems RenShape® SL 7820 Stereolithography Plastic
DSM Somos® Element Stereolithography Polymer

PDSMT027 / 93547

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.