MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
AISI 422 12Cr-1Mo-1W-0.3V HEAT RESISTING STEEL BARS FOR TURBINE BLADES (SUH 616-B)
Categories: Metal; Ferrous Metal; Stainless Steel; Cast Stainless Steel; Tool Steel; Cold Work Steel

Material Notes:

Creep and rupture data provided by NIMS

Key Words: JIS G4311(91) SUH616-B; UNS S42200
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 7.81 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Brinell 341
Tensile Strength, Ultimate 880 MPa
Tensile Strength, Yield 735 MPa
Elongation at Break 25 %
Rupture Strength 29.0 MPa
@Temperature 650 °C,
Time 3.60e+8 sec
 31.0 - 50.0 MPa
@Temperature 625 °C,
Time 3.60e+8 sec
 36.0 - 67.0 MPa
@Temperature 600 °C,
Time 3.60e+8 sec
 52.0 - 111 MPa
@Temperature 575 °C,
Time 3.60e+8 sec
 89.0 - 182 MPa
@Temperature 550 °C,
Time 3.60e+8 sec
 144 - 249 MPa
@Temperature 525 °C,
Time 3.60e+8 sec
 243 - 313 MPa
@Temperature 500 °C,
Time 3.60e+8 sec
 
Component Elements PropertiesOriginal ValueComments
Carbon, C 0.20 - 0.25 %
Chromium, Cr 11 - 12.5 %
Iron, Fe 82.54 - 86.1 %
Manganese, Mn 0.50 - 0.90 %
Molybdenum, Mo 0.50 - 0.70 %
Nickel, Ni 0.75 - 1.25 %
Phosphorus, P <= 0.030 %
Silicon, Si <= 0.40 %
Sulfur, S <= 0.030 %
Tungsten, W 0.75 - 1.1 %
Vanadium, V 0.20 - 0.30 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
AISI 403 12Cr STAINLESS STEEL BARS FOR TURBINE BLADES (SUS 403-B)
AISI Type 430F Stainless Steel soft tempered wire 6.4 mm diameter
AISI Type 410S Stainless Steel
ASTM A285, Grade A
15Cr-28Co-4Mo-2.5Ti-3Al NICKEL BASED SUPERALLOY BARS FOR GAS TURBINE BLADES

NIMS019 / 77536

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.