MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

Tropical Opepe Wood
Categories: Wood and Natural Products; Wood; Hardwood

Material Notes: Data is based on small, clear, air-dried samples unless specified.
Usual surface texture: Coarse
Dimensional changes when dried lumber is subjected to variations in humidity during service: Small
Resistance to fungal decay (Heartwood in ground contact): Very Durable (Over 25 years)
Resistance to penetration by preservatives: Moderately resistant to resistant
Common Applications: Heavy constructional work. Marine and freshwater use. Exterior joinery. Flooring

Key Words: Nauclea Diderrichii; Lumber, Timber
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 0.630 g/cc0.630 g/ccGreen, African Origin
Density 0.740 g/cc0.0267 lb/in³Air Dry (12-15% Moisture Content)
 
Mechanical PropertiesMetricEnglishComments
Hardness, Wood Indentation 6800 N1530 lb (f)Side Hardness, Green, African Origin
 7300 N1640 lb (f)Side Hardness, 12% Moisture, African Origin
Modulus of Rupture 0.0938 GPa13.6 ksiStatic Bending, Green, African Origin
 0.120 GPa17.4 ksiStatic Bending, 12% Moisture, African Origin
 0.127 GPa18.4 ksiStatic Bending
Flexural Modulus 11.9 GPa1730 ksiStatic Bending, Green, African Origin
 13.4 GPa1940 ksiStatic Bending, 12% Moisture, African Origin
 13.82 GPa2004 ksiStatic Bending
Compressive Strength 51.6 MPa7480 psiParallel to Grain, Green, African Origin
 59.0 MPa8560 psi
 71.7 MPa10400 psiParallel to Grain, 12% Moisture, African Origin
Machinability 50 %50 %Medium Relative to Other Wood
Shear Strength 13.1 MPa1900 psiParallel to Grain, Green, African Origin
 17.1 MPa2480 psiParallel to Grain, 12% Moisture, African Origin
Work to Maximum Load 0.0840 J/cm³12.2 in-lb/in³Static Bending, Green, African Origin
 0.0990 J/cm³14.4 in-lb/in³Static Bending, 12% Moisture, African Origin
Toughness 15.6 J11.5 ft-lb2 cm x 2 cm sample
 
Thermal PropertiesMetricEnglishComments
Shrinkage 4.5 %4.5 %Radial Shrinkage Green to Oven Dry, African Origin
 7.5 %7.5 %Tangential; Green to Zero Moisture
 8.4 %8.4 %Tangential Shrinkage Green to Oven Dry, African Origin
 12.6 %12.6 %Volumetric Shrinkage Green to Oven Dry, African Origin
 
Descriptive Properties
ColorYellow to orange yellowUsual for heartwood

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Tropical American Lemonwood Wood
Tropical Balsa Wood
Tropical Dark Red Meranti Wood
Tropical Obeche Wood
Tropical Sapele Wood

PTST160 / 71398

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.