MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

Latrobe LSS™ A6 Tool Steel (ASTM A6)
Categories: Metal; Ferrous Metal; Alloy Steel; Medium Alloy Steel; Tool Steel

Material Notes: TLS A6 tool steel is a medium-alloy, air-hardening tool steel that is characterized by its ability to be through hardened while using the low austenitizing temperatures which are typically associated with oil-hardening tool steels. TLS A6 exhibits good toughness and excellent dimensional stability in heat treatment. TLS A6 is intermediate in wear resistance between O1 oil-hardening tool steel and D2 high-carbon, high-chromium tool steel. Typical applications for TLS A6 tool steel include blanking and forming dies, trim dies, bending and forming tools, mandrels, chuck jaws, tooling for plastic injection molding, dowel pins, shear knives, and gages.

Information Provided by Timken Latrobe Steel.

Timken sold Latrobe in December 2006. They are now Latrobe Specialty Steels Co.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 7.83 g/cc7.83 g/cc
Density 7.83 g/cc0.283 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell C 4747Air Cooled from 843°C, 593°C Temper Temperature
 5252Air Cooled from 843°C, 427°C Temper Temperature
 6262Air Cooled from 843°C, As Quenched
Modulus of Elasticity 207 GPa30000 ksi
Machinability 80 %80 %1% Carbon Steel
Izod Impact Unnotched 40.7 J30.0 ft-lbAir Cooled from 843°C; 150°C Temper Temperature
 102 J75.0 ft-lbAir Cooled from 843°C; 316°C Temper Temperature
 
Thermal PropertiesMetricEnglishComments
CTE, linear  13.1 µm/m-°C
@Temperature 21.0 - 316 °C
7.28 µin/in-°F
@Temperature 69.8 - 601 °F
 14.7 µm/m-°C
@Temperature 21.0 - 704 °C
8.17 µin/in-°F
@Temperature 69.8 - 1300 °F
 
Processing PropertiesMetricEnglishComments
Processing Temperature 727 °C1340 °FCritical Temperaure Ac1
 
Component Elements PropertiesMetricEnglishComments
Carbon, C 0.70 %0.70 %
Chromium, Cr 1.0 %1.0 %
Iron, Fe 94.75 %94.75 %
Manganese, Mn 2.0 %2.0 %
Molybdenum, Mo 1.25 %1.25 %
Silicon, Si 0.30 %0.30 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
ASTM A131 Steel, Grade AH36
AISI Type A6 Tool Steel
AISI Type A2 Tool Steel
AISI Type S1 Tool Steel, quenched 955°C (1750°F), tempered 150°C (300°F)
ASTM A353 Alloy Steel

NTIMK100 / 19447

Free Trade Publications, Click Here!
Free Trade Publications, Click Here!

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.