MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
Latrobe Lescalloy® 410Cb High Strength Stainless Steel
Categories: Metal; Ferrous Metal; Stainless Steel

Material Notes: LESCALLOY 17-4 VAC-ARC steel is a precipitation hardening martensitic stainless steel. A wide range of mechanical properties is available via simple aging within a 900-1150°F (482-621°C) temperature range. Vacuum arc remelting provides low gas content, superior cleanliness and optimum transverse properties.

Information Provided by Timken Latrobe Steel.

Timken sold Latrobe in December 2006. They are now Latrobe Specialty Steels Co.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 7.75 g/cc
Density 0.280 lb/in³
 
Mechanical PropertiesOriginal ValueComments
Hardness, Brinell 2554 in. Test Specimen
 2555.25 in. Test Specimen
Tensile Strength, Ultimate 123 ksi5.25 in. Test Specimen
 124 ksi4 in. Test Specimen
Tensile Strength, Yield 724 MPa
@Strain 0.2 %
5.25 in. Test Specimen
 731 MPa
@Strain 0.2 %
4 in. Test Specimen
Elongation at Break 21 %4 in. Test Specimen
 22 %5.25 in. Test Specimen
Reduction of Area 65 - 66 %4 in. Test Specimen
 66 %5.25 in. Test Specimen
Modulus of Elasticity 29000 ksi
Machinability 50 - 55 %Mild Steel
Charpy Impact 60.0 JV-Notch; 5.25 in. Test Specimen
 98.0 JV-Notch; 4 in. Test Specimen
 
Thermal PropertiesOriginal ValueComments
CTE, linear 10.1 µm/m-°C
@Temperature 21.0 - 204 °C
 12.1 µm/m-°C
@Temperature 20.0 - 649 °C
Specific Heat Capacity 0.110 BTU/lb-°F
@Temperature 0.000 - 100 °C
Thermal Conductivity 25.0 W/m-K
@Temperature 100 °C
 
Component Elements PropertiesOriginal ValueComments
Carbon, C 0.13 %
Chromium, Cr 11.6 %
Iron, Fe 86.79 %
Manganese, Mn 0.50 %
Nickel, Ni 0.60 %
Niobium, Nb (Columbium, Cb) 0.080 %
Silicon, Si 0.30 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Latrobe Lescalloy® AF 1410 VIM-VAR ; 6 in High Strength Alloy Steel
Latrobe Lescalloy® 300M - HS VAC-ARC High Strength Alloy Steel
329 Stainless Steel, annealed strip
329 Stainless Steel, annealed bar
420 Stainless Steel, annealed and cold drawn bar

NTIMK060 / 19407

Free Trade Publications, Click Here!
Free Trade Publications, Click Here!

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.