MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

Chemours Viton® B-202 with 2.5 phr N990 Carbon Black
Categories: Polymer; Thermoset; Fluoropolymer, TS; Thermoset Fluoroelastomer; Rubber or Thermoset Elastomer (TSE)

Material Notes: Viton® B-202 is a low viscosity, B-type gum polymer that demonstrates improved processing and rheology when compared with existing fluoroelastomers. Viton® B-202 is designed to be cured with either Viton® Curative #30 or Viton® Curative #50. When using Viton® Curative #30, use Viton® Curative #20 in a ratio of about 1.8 Viton® Curative #30 to Viton® Curative #20. When using Viton® Curative #50, use 0.3–0.5 phr of Viton® Curative #20 to ensure a fast cure rate. Note that Viton® Curative #20 can be difficult to mix into low viscosity stocks, such as those based on Viton® B-202, and careful attention needs to be paid to mixing procedures. Compared with other B-family terpolymers, Viton® B-202 provides:
  • Low viscosity
  • Improved processing
  • Increased mold flow
  • Excellent mold release

Applications:

  • Transfer and injection molding of complex shapes
  • Extrusions (e.g., fuel hose and tubing)
  • Solution coatings of fabrics, tanks or chemical containers

Viton® B-202 can be blended with other Viton® types to modify viscosity, enhance processability and/or improve flow.

Information provided by manufacturer.

Chemours was formed from former DuPont performance chemicals businesses, including the Viton product line, in 2015.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Mooney Viscosity 41
@Temperature 121 °C
41
@Temperature 250 °F
ML 1 + 10
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A 5656Cured 10 min at 177°C and Post Cured 24 hr at 232°C
Tensile Strength, Ultimate 8.40 MPa1220 psiCured 10 min at 177°C and Post Cured 24 hr at 232°C
Elongation at Break 295 %295 %Cured 10 min at 177°C and Post Cured 24 hr at 232°C
100% Modulus 1.60 MPa
@Strain 100 %
232 psi
@Strain 100 %
Cured 10 min at 177°C and Post Cured 24 hr at 232°C
Compression Set 26 %
@Temperature 200 °C
26 %
@Temperature 392 °F
Method B, Plied Disks, 70 hr
 
Descriptive Properties
Formulation as Tested0.5Viton® Curative No. 20
 2.5MT Black (N-990)
 2.5Viton® Curative No. 50
 3High-Activity MgO
 6Calcium Hydroxide
 97Viton® B-202

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
LG Chemical NBR 7030 High Acrylonitrile Polymer
Chemours Viton® A-331C with Albaglos Fluoroelastomer Compound
Chemours Viton® A-331C with 60 MT Black Fluoroelastomer Compound
Chemours Viton® B-202 with 45 phr N990 Carbon Black
Dow Nordel® IP 4570 Radiator/Heater Hose

PDVDA31 / 34000

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.