MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

(Viewing data as-entered. Click here to return)
Eastman Eastar™ Renew EN001-25 Copolyester
Categories: Polymer; Thermoplastic; Polyester, TP

Material Notes: Eastar Renew EN001-25 is a clear copolyester for single use food & beverage and general purpose packaging. It is designed for injection stretch blow molding (ISBM) and has enhanced processing capability compared to commodity PET. Eastman Renew polymers have been certified by International Sustainability & Carbon Certification (ISCC), a global, independent agency for tracking sustainable content in a variety of industries. Renew polymers are produced with ISCC certified circular content by mass balance allocation. Eastar Renew Copolyester EN001-25 meets the definition of resin identification code #1 (RIC1) as defined by ASTM D7611. Other end product attributes including but not limited to size, color, auxiliary components, and availability of collection may impact recyclability. Eastar Renew Copolyester EN001-25 may be used in various food contact applications under the U.S. Food & Drug Administration (FDA) regulations. This product has been GREENGUARD INDOOR AIR QUALITY CERTIFIED. The GREENGUARD INDOOR AIR QUALITY CERTIFIED mark is a registered certification mark used under license through the GREENGUARD Environmental Institute (GEI). GEI is an industry-independent, non-profit organization that oversees the GREENGUARD Certification Program. The GREENGUARD Certification Program is an industry independent, third-party testing program for low-emitting products and materials for indoor environments. For more information about GEI and to obtain printable certificates for Eastman copolyesters, visit www.greenguard.org. Choose Eastman Chemical Company under the Manufacturer category and click search to display a list of our products.

Applications

  • Blow molding
  • Flavored water packaging
  • Fruit juice drinks packaging
  • Personal care packaging
  • Soft drink packaging
  • Sport drinks packaging
  • Still water packaging
Key Attributes
  • Clear appearance
  • Enhanced processing capability compared to commodity PET
  • Good for injection stretch blow molding (ISBM)
  • Not a material of concern
  • PVC alternative
  • Recyclable

Information provided by Eastman.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.33 g/ccASTM D792
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell R 112ASTM D785
 114ISO 2039-2
Tensile Strength at Break 25.0 MPaASTM D638
 25.0 MPaISO 527
Tensile Strength, Yield 57.0 MPaISO 527
 58.0 MPaASTM D638
Elongation at Break 120 %ASTM D638
 120 %ISO 527
Tensile Modulus 2400 MPaASTM D638
 2400 MPaISO 527
Flexural Yield Strength 77.0 MPaISO 178
 84.0 MPaASTM D790
Flexural Modulus 2300 MPaISO 178
 2500 MPaASTM D790
Izod Impact, Notched 27.0 J/m
@Temperature -40.0 °C
ASTM D256
 40.0 J/m
@Temperature 23.0 °C
ASTM D256
Izod Impact, Unnotched NB
@Temperature -20.0 °C
ASTM D4812
 NB
@Temperature 23.0 °C
ASTM D4812
 NB
@Temperature -30.0 °C
ASTM D4812
 NB
@Temperature -40.0 °C
ASTM D4812
Izod Impact, Notched (ISO) 3.10 kJ/m²
@Temperature -40.0 °C
Type 1 Specimen, Type A Notch; ISO 180
 4.50 kJ/m²
@Temperature 23.0 °C
Type 1 Specimen, Type A Notch; ISO 180
Izod Impact, Unnotched (ISO) 170 kJ/m²
@Temperature -40.0 °C
Type 1 Specimen; ISO 180
 190 kJ/m²
@Temperature -30.0 °C
Type 1 Specimen; ISO 180
 NB
@Temperature -20.0 °C
Type 1 Specimen; ISO 180
 NB
@Temperature 23.0 °C
Type 1 Specimen; ISO 180
Puncture Energy 0.800 J
@Temperature -40.0 °C
Energy @ Max. Load, 2.5 mm (0.100 in.) Thick Plaques; ISO 6603-2
 1.00 J
@Temperature -40.0 °C
Energy @ Max. Load, 3.2 mm (0.125 in.) Thick Plaques; ISO 6603-2
 1.60 J
@Temperature -40.0 °C
Energy @ Max. Load, 2.5 mm (0.100 in.) Thick Plaques; ASTM D3763
 2.10 J
@Temperature -40.0 °C
Energy @ Max. Load, 3.2 mm (0.125 in.) Thick Plaques; ASTM D3763
 15.0 J
@Temperature 23.0 °C
Energy @ Max. Load, 2.5 mm (0.100 in.) Thick Plaques; ISO 6603-2
 18.0 J
@Temperature 23.0 °C
Energy @ Max. Load, 3.2 mm (0.125 in.) Thick Plaques; ISO 6603-2
 26.0 J
@Temperature 23.0 °C
Energy @ Max. Load, 2.5 mm (0.100 in.) Thick Plaques; ASTM D3763
 31.0 J
@Temperature 23.0 °C
Energy @ Max. Load, 3.2 mm (0.125 in.) Thick Plaques; ASTM D3763
 
Thermal PropertiesOriginal ValueComments
Deflection Temperature at 0.46 MPa (66 psi) 69.0 °CASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 65.0 °CASTM D648
 
Optical PropertiesOriginal ValueComments
Haze 1.00 %ASTM D1003
Transmission, Visible 84.0 %Total; ASTM D1003
 
Compliance PropertiesOriginal ValueComments
FDA YesSee notes for details

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PEATM4125 / 323748

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.