MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
HK40 CENTRIFUGALLY CAST 25Cr-20Ni-0.4C STEEL TUBES FOR USE IN REFORMER FURNACES (SCH 22-CF)
Categories: Metal; Ferrous Metal; Superalloy

Material Notes:

Creep and rupture data provided by NIMS

Key Words: UNS J94204; JIS G5122(91) SCH 22-CF; ASTM A351(94); ASTM A608(98)
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength, Ultimate 440 MPa
Tensile Strength, Yield 235 MPa
Elongation at Break 8.0 %
Rupture Strength 6.00 - 7.00 MPa
@Temperature 975 °C,
Time 3.60e+8 sec
 6.00 - 8.00 MPa
@Temperature 950 °C,
Time 3.60e+8 sec
 7.00 - 10.0 MPa
@Temperature 925 °C,
Time 3.60e+8 sec
 9.00 - 12.0 MPa
@Temperature 900 °C,
Time 3.60e+8 sec
 11.0 - 15.0 MPa
@Temperature 875 °C,
Time 3.60e+8 sec
 13.0 - 18.0 MPa
@Temperature 850 °C,
Time 3.60e+8 sec
 16.0 - 22.0 MPa
@Temperature 825 °C,
Time 3.60e+8 sec
 19.0 - 27.0 MPa
@Temperature 800 °C,
Time 3.60e+8 sec
 
Component Elements PropertiesOriginal ValueComments
Carbon, C 0.35 - 0.45 %
Chromium, Cr 23 - 27 %
Iron, Fe 46.72 - 57.65 %
Manganese, Mn <= 1.5 %
Molybdenum, Mo <= 0.50 %
Nickel, Ni 19 - 22 %
Phosphorus, P <= 0.040 %
Silicon, Si <= 1.75 %
Sulfur, S <= 0.040 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Cast Stainless Steel HK40, ASTM A351M
MetalTek MTEK HK40 Cast UNS J94204 Heat Resistant Stainless Steel
Cast Stainless Steel HK40, ACI
Cast Stainless Steel HK40, ASTM A608
AFE Technologies Cronite 25Cr/20Ni No. HR6

NIMS029 / 77546

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.