MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

MOL Group TATREN IM 100 85 PP, Impact copolymer for injection molding
Categories: Polymer; Thermoplastic; Polypropylene (PP); Polypropylene, Impact Modified; Molded/Extruded

Material Notes: Description: TATREN IM 100 85 is a reactor impact copolymer of exceptionally high fluidity and excellent processability. This grade contains nucleating and antistatic agent. TATREN IM 100 85 is characterized by high stiffness and good impact resistance. This grade has excellent organoleptic properties which makes it suitable to be used for food contact applications.

Applications: TATREN IM 100 85 is intended especially for very high speed thin wall injection molding of products where high stiffness and good impact resistance is required. Typical end products are household and garden articles like bowls, pails, storage boxes, trays, caps, closures, boxes for food packaging etc. This grade can be used in mixtures with TATREN homopolymer grades.

(1) Typical properties measured on standard injection molded test specimen according to ISO 294-1.

Information provided by Molgroup Chemicals

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Melt Flow 100 g/10 min
@Load 2.16 kg,
Temperature 230 °C
100 g/10 min
@Load 4.76 lb,
Temperature 446 °F
ISO 1133-1
Storage Temperature <= 40.0 °C<= 104 °F
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell R 80801; ISO 2039-2
Tensile Strength, Yield 23.0 MPa3340 psi1; ISO 527-1,2
Elongation at Yield 4.0 %4.0 %1; ISO 527-1,2
Modulus of Elasticity 1.40 GPa203 ksi1, in Tension; ISO 527-1,2
Flexural Modulus 1.35 GPa196 ksi1; ISO 178
Izod Impact, Notched (ISO)  3.00 kJ/m²
@Temperature -20.0 °C
1.43 ft-lb/in²
@Temperature -4.00 °F
1; ISO 180/A
 4.50 kJ/m²
@Temperature 23.0 °C
2.14 ft-lb/in²
@Temperature 73.4 °F
1; ISO 180/A
 
Thermal PropertiesMetricEnglishComments
Deflection Temperature at 0.46 MPa (66 psi) 92.0 °C198 °F1, flatwise; ISO 75-1,2
 
Processing PropertiesMetricEnglishComments
Processing Temperature 190 - 250 °C374 - 482 °F

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PMOLG105 / 297271

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.