MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger PEI

Ascend Performance Materials Vydyne® 47H Nylon 66, Impact Modified, Conditioned  (Unverified Data**)
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 66 (PA66); Nylon 66, Impact Grade

Material Notes: Vydyne® 47H is general-purpose, impact-modified PA66 resin. Available in natural, it is heat-stabilized for improved resistance to elevated temperatures. The heat stabilization package for Vydyne 47H was formulated to provide thermal endurance when used in applications in which continuous or extended high-temperature exposure is anticipated. Vydyne 47H is recognized for all the processing and property advantages inherent to PA66 with the addition of improved impact strength. This resin offers a well balanced combination of engineering properties characterized by high melt point, good surface lubricity, abrasion resistance and resistance to many chemicals, machine and motor oils, solvents and gasoline. Vydyne 47H is designed to meet the critical low-temperature impact requirements called out in many automotive specifications.

Availability:

  • Asia Pacific
  • Europe
  • North America
Additive:
  • Impact Modifier
Features:
  • Gasoline Resistance
  • General Purpose
  • Good Abrasion Resistance
  • Good Chemical Resistance
  • Good Processability
  • Good Toughness
  • High Impact Resistance
  • Impact Modified
  • Low Temperature Impact Resistance
  • Low Temperature Toughness
  • Oil Resistant
  • Solvent Resistant
Uses:
  • Automotive Applications
  • Connectors
  • Consumer Applications
  • Electrical/Electronic Applications
  • Fasteners
  • Gears
  • Industrial Applications
Appearance: Natural Color

Forms: Pellets

Processing Method: Injection Molding

Information provided by Ascend Performance Materials.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.10 g/cc0.0397 lb/in³ISO 1183
Water Absorption 1.2 %
@Time 86400 sec
1.2 %
@Time 24.0 hour
ISO 62
Moisture Absorption at Equilibrium 2.3 %2.3 %50% RH; ISO 62
Linear Mold Shrinkage, Flow 0.018 cm/cm
@Diameter 2.00 mm
0.018 in/in
@Diameter 0.0787 in
ISO 294-4
Linear Mold Shrinkage, Transverse 0.016 cm/cm
@Diameter 2.00 mm
0.016 in/in
@Diameter 0.0787 in
ISO 294-4
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 40.0 MPa5800 psiISO 527-2
Tensile Strength, Yield 45.0 MPa6530 psiISO 527-2
Elongation at Break >= 60 %>= 60 %ISO 527-2
Tensile Modulus 1.74 GPa252 ksiISO 527-2
Flexural Strength 24.0 MPa3480 psiISO 178
Flexural Modulus 0.780 GPa113 ksiISO 178
Izod Impact, Notched (ISO)  18.0 kJ/m²
@Temperature -40.0 °C
8.57 ft-lb/in²
@Temperature -40.0 °F
ISO 180
 24.0 kJ/m²
@Temperature -30.0 °C
11.4 ft-lb/in²
@Temperature -22.0 °F
ISO 180
 44.0 kJ/m²
@Temperature 23.0 °C
20.9 ft-lb/in²
@Temperature 73.4 °F
ISO 180
Charpy Impact Unnotched  NB
@Temperature -30.0 °C
NB
@Temperature -22.0 °F
ISO 179
 NB
@Temperature 23.0 °C
NB
@Temperature 73.4 °F
ISO 179
Charpy Impact, Notched  1.80 J/cm²
@Temperature -40.0 °C
8.57 ft-lb/in²
@Temperature -40.0 °F
ISO 179
 2.40 J/cm²
@Temperature -30.0 °C
11.4 ft-lb/in²
@Temperature -22.0 °F
ISO 179
 6.20 J/cm²
@Temperature 23.0 °C
29.5 ft-lb/in²
@Temperature 73.4 °F
ISO 179

**
This data sheet is not an active part of MatWeb and the information on it should not be considered reliable.
Inactive data sheets have usually been replaced with newer information on the same material. If this is the case, you can find the active data sheet by using any of our search tools, including the Quick Search box in the upper part of this page.
If you are unable to locate an active data sheet for this material, then this material is likely discontinued, although various other reasons may be behind its removal. In any event, do not rely on the information on this page to be accurate or maintained.
You may have reached this data sheet through an outdated bookmark or link. Please update your bookmark accordingly. We apologize if you have accessed this page through MatWeb’s usual search tools.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PZVYDYM889 / 177240

Visit Zeus Inc. for PEEK Tubing

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.