MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Epoxies, Etc 10-3008 Flexible Structural Epoxy Adhesive
Categories: Polymer; Thermoset; Epoxy; Epoxy Adhesive

Material Notes: Description: 10-3008 is a filled, high performance structural epoxy adhesive. 10-3008 is a flexible adhesive with outstanding lap shear and peel strength. It is a great choice for bonding substrates of differing coefficients of thermal expansion. 10-3008 is also an excellent adhesive for applications requiring impact and vibration resistance. 10-3008 has a convenient 1:1 by volume mix ratio and therefore is ideal for Dual Barrel Cartridge packaging. 10-3008 is stocked in 50ML and 200ML Dual Cartridge sizes. 10-3008 contains non-abrasive fillers and therefore is well suited for meter mix and dispense equipment.

Features:

  • 1:1 Non-critical mix ratio
  • High lap shear strength
  • Thermal shock resistance
  • Excellent chemical resistance

Information provided by Epoxies, Etc

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.23 g/cc1.23 g/ccCatalyst
 1.69 g/cc1.69 g/ccResin
Viscosity 77867 cP77867 cPCatalyst
 96000 cP96000 cPMixed
 650000 cP650000 cPResin
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore D 55 - 6555 - 65
Shear Strength 20.7 MPa3000 psiLap (AL/AL), 18 hours + 2 hours @ 212°F
 18.6 MPa
@Temperature 121 °C,
Time 1800 sec
2700 psi
@Temperature 250 °F,
Time 0.500 hour
Lap (AL/AL)
 20.0 MPa
@Temperature 25.0 °C,
Time 605000 sec
2900 psi
@Temperature 77.0 °F,
Time 168 hour
Lap (AL/AL)
 20.7 MPa
@Temperature 82.0 °C,
Time 3600 sec
3000 psi
@Temperature 180 °F,
Time 1.00 hour
Lap (AL/AL)
 22.1 MPa
@Temperature 65.6 °C,
Time 7200 sec
3200 psi
@Temperature 150 °F,
Time 2.00 hour
Lap (AL/AL)
Peel Strength 4.38 kN/m25.0 pli18 hours + 2 hours @ 212°F
 4.03 kN/m
@Temperature 82.0 °C,
Time 3600 sec
23.0 pli
@Temperature 180 °F,
Time 1.00 hour
 4.03 kN/m
@Temperature 121 °C,
Time 1800 sec
23.0 pli
@Temperature 250 °F,
Time 0.500 hour
 4.38 kN/m
@Temperature 25.0 °C,
Time 605000 sec
25.0 pli
@Temperature 77.0 °F,
Time 168 hour
 4.56 kN/m
@Temperature 65.6 °C,
Time 7200 sec
26.0 pli
@Temperature 150 °F,
Time 2.00 hour
 
Processing PropertiesMetricEnglishComments
Cure Time  0.500 min
@Temperature 121 °C
0.00833 hour
@Temperature 250 °F
 60.0 min
@Temperature 65.6 °C
1.00 hour
@Temperature 150 °F
 120 min
@Temperature 82.0 °C
2.00 hour
@Temperature 180 °F
 1080 - 1440 min
@Temperature 25.0 °C
18.0 - 24.0 hour
@Temperature 77.0 °F
Pot Life 60.0 min
@Load 0.100 kg
60.0 min
@Load 0.221 lb
Shelf Life 12.0 Month12.0 Month
 
Descriptive Properties
ColorBeigeCatalyst
 GreyResin
Mix Ratio1:1by volume (Resin:Catalyst)
 1:1.3by weight (Resin:Catalyst)

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PFEPOX077 / 316754

Master Bond adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.