MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

Haynes Hastelloy® C-22HS® Nickel Alloy Plate and Bar, Hot-rolled, Solution Annealed, Age-hardened
Categories: Metal; Nonferrous Metal; Nickel Alloy

Material Notes: Outstanding Corrosion Resistance, High Strength

HASTELLOY® C-22HSTM alloy is corrosion-resistant, nickel-chromium-molybdenum alloy which can be heat treated to obtain a strength approximately double that of other C-type alloys. Importantly, the corrosion resistance and ductility of the alloy remain excellent when in the high strength condition. In addition to its high uniform corrosion resistance in oxidizing as well as reducing environments, the as-heat treated C-22HS alloy possesses high resistance to chloride-induced pitting and crevice corrosion attack.

C-22HS alloy is available in the form of plate, sheet, strip, billet, bar, wire, pipe, and tube.

Heat Treatment: The high strength of C-22HS alloy is derived from the formation of strengthening particles of Ni2(Mo,Cr) which form during the patented two-step age-hardening heat treatment. The approximately 48 hour heat treatment, 1300°F (705°C) FC to 1125°F (605°C)/32 hours/AC, is described in more detail on page 14.

Solution Annealed and Filler Wire Applications: C-22HS alloy may also be considered for applications which do not require the high strength imparted by the heat treatment. In the annealed condition, C-22HS alloy has even higher corrosion-resistance, particularly with regard to localized corrosive attack. This localized attack resistance also makes the alloy an attractive candidate as a general-purpose filler metal or weld overlay.

Applications:

  • Agitators and blenders
  • Shafting
  • Fan blades and hubs
  • Fasteners
  • Springs
  • Valves
  • Dies
  • Screws
  • Wellhead parts
  • Rings and gaskets

Heat Treatment: Wrought forms of C-22HS alloy are furnished in the solution annealed condition, unless otherwise specified. The standard solution annealing treatment consists of heating to 1975°F (1080°C) followed by rapid air-cooling or water quenching. Parts which have been hot formed should be solution annealed prior to final fabrication or installation. To use the alloy in the high-strength condition, it is necessary to age-harden using a two step treatment of 1300°F (705°C) for 16 hours, furnace cooling to 1125°F (605°C) and holding at that temperature for 32 hours, followed by an air cool. Cold or hot-worked structures should normally be given a full solution anneal prior to performing the age-hardening treatment.

Forming: C-22HS alloy has excellent forming characteristics, and cold forming is the preferred method of shaping. The alloy can be easily cold worked due to its good ductility. The alloy is generally stiffer than the austenitic stainless steels; therefore more energy is required during cold forming.

Machining: C-22HS alloy may be machined in either the solution annealed or age-hardened condition. Carbide or ceramic tools are recommended. For use in the age-hardened condition, it is suggested to rough machine in the annealed condition. After performing the age-hardening heat treatment, light machining may be performed to achieve desired final dimensions.

Data provided by the manufacturer, Haynes International, Inc.

Vendors: Visit metalmen for your metals needs. Products include special chemistry, tight tolerances, custom tempers, odd dimensions/forms, and small quantities. Phone 1-800-767-9494.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 8.60 g/cc0.311 lb/in³annealed
 8.64 g/cc0.312 lb/in³age-hardened
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Ultimate  902 MPa
@Temperature 600 °C
131000 psi
@Temperature 1110 °F
 964 MPa
@Temperature 500 °C
140000 psi
@Temperature 932 °F
 1006 MPa
@Temperature 400 °C
145900 psi
@Temperature 752 °F
 1047 MPa
@Temperature 300 °C
151900 psi
@Temperature 572 °F
 1089 MPa
@Temperature 200 °C
157900 psi
@Temperature 392 °F
 1153 MPa
@Temperature 100 °C
167200 psi
@Temperature 212 °F
 1202 MPa
@Temperature 25.0 °C
174300 psi
@Temperature 77.0 °F
Tensile Strength, Yield  488 MPa
@Strain 0.2 %,
Temperature 600 °C
70800 psi
@Strain 0.2 %,
Temperature 1110 °F
 507 MPa
@Strain 0.2 %,
Temperature 500 °C
73500 psi
@Strain 0.2 %,
Temperature 932 °F
 518 MPa
@Strain 0.2 %,
Temperature 400 °C
75100 psi
@Strain 0.2 %,
Temperature 752 °F
 539 MPa
@Strain 0.2 %,
Temperature 300 °C
78200 psi
@Strain 0.2 %,
Temperature 572 °F
 579 MPa
@Strain 0.2 %,
Temperature 200 °C
84000 psi
@Strain 0.2 %,
Temperature 392 °F
 627 MPa
@Strain 0.2 %,
Temperature 100 °C
90900 psi
@Strain 0.2 %,
Temperature 212 °F
 690 MPa
@Strain 0.2 %,
Temperature 25.0 °C
100000 psi
@Strain 0.2 %,
Temperature 77.0 °F
Elongation at Break  44.2 %
@Temperature 25.0 °C
44.2 %
@Temperature 77.0 °F
 47.7 %
@Temperature 100 °C
47.7 %
@Temperature 212 °F
 48.3 %
@Temperature 200 °C
48.3 %
@Temperature 392 °F
 49.2 %
@Temperature 600 °C
49.2 %
@Temperature 1110 °F
 50.3 %
@Temperature 500 °C
50.3 %
@Temperature 932 °F
 52.3 %
@Temperature 400 °C
52.3 %
@Temperature 752 °F
 52.7 %
@Temperature 300 °C
52.7 %
@Temperature 572 °F
Reduction of Area  55.7 %
@Temperature 100 °C
55.7 %
@Temperature 212 °F
 57.7 %
@Temperature 25.0 °C
57.7 %
@Temperature 77.0 °F
 60 %
@Temperature 200 °C
60 %
@Temperature 392 °F
 63.2 %
@Temperature 500 °C
63.2 %
@Temperature 932 °F
 63.4 %
@Temperature 400 °C
63.4 %
@Temperature 752 °F
 63.9 %
@Temperature 300 °C
63.9 %
@Temperature 572 °F
 66.9 %
@Temperature 600 °C
66.9 %
@Temperature 1110 °F
Modulus of Elasticity  181 GPa
@Temperature 600 °C
26300 ksi
@Temperature 1110 °F
Dynamic
 195 GPa
@Temperature 500 °C
28300 ksi
@Temperature 932 °F
Dynamic
 205 GPa
@Temperature 400 °C
29700 ksi
@Temperature 752 °F
Dynamic
 209 GPa
@Temperature 300 °C
30300 ksi
@Temperature 572 °F
Dynamic
 211 GPa
@Temperature 200 °C
30600 ksi
@Temperature 392 °F
Dynamic
 218 GPa
@Temperature 100 °C
31600 ksi
@Temperature 212 °F
Dynamic
 223 GPa
@Temperature 25.0 °C
32300 ksi
@Temperature 77.0 °F
Dynamic
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity  0.0000980 ohm-cm
@Temperature 25.0 °C
0.0000980 ohm-cm
@Temperature 77.0 °F
 0.000100 ohm-cm
@Temperature 100 °C
0.000100 ohm-cm
@Temperature 212 °F
 0.000104 ohm-cm
@Temperature 200 °C
0.000104 ohm-cm
@Temperature 392 °F
 0.000108 ohm-cm
@Temperature 300 °C
0.000108 ohm-cm
@Temperature 572 °F
 0.000112 ohm-cm
@Temperature 400 °C
0.000112 ohm-cm
@Temperature 752 °F
 0.000115 ohm-cm
@Temperature 500 °C
0.000115 ohm-cm
@Temperature 932 °F
 0.000117 ohm-cm
@Temperature 600 °C
0.000117 ohm-cm
@Temperature 1110 °F
 
Thermal PropertiesMetricEnglishComments
CTE, linear  11.6 µm/m-°C
@Temperature 25.0 - 100 °C
6.44 µin/in-°F
@Temperature 77.0 - 212 °F
 12.0 µm/m-°C
@Temperature 25.0 - 200 °C
6.67 µin/in-°F
@Temperature 77.0 - 392 °F
 12.4 µm/m-°C
@Temperature 25.0 - 300 °C
6.89 µin/in-°F
@Temperature 77.0 - 572 °F
 12.7 µm/m-°C
@Temperature 25.0 - 400 °C
7.06 µin/in-°F
@Temperature 77.0 - 752 °F
 13.1 µm/m-°C
@Temperature 25.0 - 500 °C
7.28 µin/in-°F
@Temperature 77.0 - 932 °F
 13.3 µm/m-°C
@Temperature 25.0 - 600 °C
7.39 µin/in-°F
@Temperature 77.0 - 1110 °F
Specific Heat Capacity  0.412 J/g-°C
@Temperature 25.0 °C
0.0985 BTU/lb-°F
@Temperature 77.0 °F
 0.434 J/g-°C
@Temperature 100 °C
0.104 BTU/lb-°F
@Temperature 212 °F
 0.451 J/g-°C
@Temperature 200 °C
0.108 BTU/lb-°F
@Temperature 392 °F
 0.465 J/g-°C
@Temperature 300 °C
0.111 BTU/lb-°F
@Temperature 572 °F
 0.477 J/g-°C
@Temperature 400 °C
0.114 BTU/lb-°F
@Temperature 752 °F
 0.488 J/g-°C
@Temperature 500 °C
0.117 BTU/lb-°F
@Temperature 932 °F
 0.504 J/g-°C
@Temperature 600 °C
0.120 BTU/lb-°F
@Temperature 1110 °F
Thermal Conductivity  11.8 W/m-K
@Temperature 25.0 °C
81.9 BTU-in/hr-ft²-°F
@Temperature 77.0 °F
 13.5 W/m-K
@Temperature 100 °C
93.7 BTU-in/hr-ft²-°F
@Temperature 212 °F
 15.4 W/m-K
@Temperature 200 °C
107 BTU-in/hr-ft²-°F
@Temperature 392 °F
 17.1 W/m-K
@Temperature 300 °C
119 BTU-in/hr-ft²-°F
@Temperature 572 °F
 18.6 W/m-K
@Temperature 400 °C
129 BTU-in/hr-ft²-°F
@Temperature 752 °F
 20.5 W/m-K
@Temperature 500 °C
142 BTU-in/hr-ft²-°F
@Temperature 932 °F
 22.4 W/m-K
@Temperature 600 °C
155 BTU-in/hr-ft²-°F
@Temperature 1110 °F
Melting Point 1304 - 1368 °C2379 - 2494 °F
Solidus 1304 °C2379 °F
Liquidus 1368 °C2494 °F
 
Processing PropertiesMetricEnglishComments
Annealing Temperature 1079 °C1975 °FFollowed by rapid air cooling or water quench
Aging Temperature  607.2 °C
@Time 115000 sec
1125 °F
@Time 32.0 hour
Age Hardening Step 2, follow by air cooling
 704 °C
@Time 57600 sec
1300 °F
@Time 16.0 hour
Age Hardening Step 1; then furnace cool to step 2
 
Component Elements PropertiesMetricEnglishComments
Aluminum, Al <= 0.50 %<= 0.50 %
Boron, B <= 0.0060 %<= 0.0060 %
Carbon, C <= 0.010 %<= 0.010 %
Chromium, Cr 21 %21 %
Cobalt, Co <= 1.0 %<= 1.0 %
Iron, Fe <= 2.0 %<= 2.0 %
Manganese, Mn <= 0.80 %<= 0.80 %
Molybdenum, Mo 17 %17 %
Nickel, Ni 57 %57 %as balance
Silicon, Si <= 0.080 %<= 0.080 %
Tungsten, W <= 1.0 %<= 1.0 %
 
Descriptive Properties
Thermal Diffusivity0.0334 cm2/sat 25°C
 0.0362 cm2/sat 100°C
 0.0398 cm2/sat 200°C
 0.0427 cm2/sat 300°C
 0.0454 cm2/sat 400°C
 0.0489 cm2/sat 500°C
 0.0517 cm2/sat 600°C

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Haynes Hastelloy® C-22HS® Nickel Alloy Plate and Bar, Hot-rolled, Solution Annealed
Latrobe MP35N® Alloy
Haynes Hastelloy® B-3® alloy, 0% cold work
AISI Type S45500 Stainless Steel, annealed at 815°C (1500°F) for 30 minutes, water quenched, bar
Haynes Hastelloy® C-22HS® Nickel Alloy Plate, Age-hardened

NHAY936 / 162630

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.