MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
AGC AFLAS® PM-1100 TFE/P Perfluoroelastomer
Categories: Polymer; Thermoset; Fluoropolymer, TS; Thermoset Fluoroelastomer; Rubber or Thermoset Elastomer (TSE)

Material Notes: Description: AFLAS® FFKM Series is a new perfluoroelastomer product line classified as an FFKM. AFLAS PM-1100 is an elastomer having the chemical structure derived from tetrafluoroethylene and perfluoroalkylvinylether. This chemical structure offers outstanding resistance to chemicals, oils, solvents, and more. PM-1100 is a peroxide-curable perfluoroelastomer.

Material Features:

  • Outstanding chemical resistance
  • Superior oil resistance
  • Outstanding solvent resistance
  • Excellent compression set
  • Exceptional mechanical strength
  • Excellent processability
End User Benefits:
  • Highly suitable for extremely harsh and aggressive chemical environments
  • Hot service temperature at 230°C, with peak exposure of 250°C
  • Can be compounded to be highly resistant to rapid gas decompression (e.g. NORSOK)
Typical Applications:
  • O-rings
  • Gaskets
  • Oilfield parts
  • Semiconductor parts

Information provided by AGC Chemicals Americas Inc.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 2.05 g/cc
Mooney Viscosity 80
@Temperature 121 °C
ML1+4
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore A 74
 74
@Treatment Temp. 230 °C,
Time 605000 sec
Heat Resistance
 75
@Treatment Temp. 200 °C,
Time 3.60e+6 sec
Heat Resistance
Tensile Strength 24.5 MPa
 22.785 MPa
@Treatment Temp. 200 °C,
Time 3.60e+6 sec
Heat Resistance
 23.275 MPa
@Treatment Temp. 230 °C,
Time 605000 sec
Heat Resistance
Elongation at Break 200 %
 266 %
@Treatment Temp. 200 °C,
Time 3.60e+6 sec
Heat Resistance
 278 %
@Treatment Temp. 230 °C,
Time 605000 sec
Heat Resistance
Tensile Modulus 0.480 MPa
@Frequency 1 Hz,
Temperature 100 °C
Storage Modulus
100% Modulus 0.00750 GPa
@Strain 100 %
Compression Set 9.6 %
@Temperature 200 °C,
Time 252000 sec
ASTM-type 1 button
 18 %
@Temperature 200 °C,
Time 252000 sec
O-ring
 29 %
@Temperature 230 °C,
Time 252000 sec
O-ring
 
Thermal PropertiesOriginal ValueComments
Maximum Service Temperature, Air 230 °C
 250 °Cpeak
 
Processing PropertiesOriginal ValueComments
Cure Time 1.10 min
@Temperature 150 °C
10% Cure, 100CPM, 3° Strain, 12 minutes by RPA-2000
 4.00 hour
@Temperature 250 °C
Post Cure
 5.00 min
@Temperature 150 °C
90% Cure, 100CPM, 3° Strain, 12 minutes by RPA-2000
 20.0 min
@Temperature 150 °C
Press cure
 
Descriptive Properties
AppearanceTranslucent white
Cure Data137.9 dNmMax S', 150°C, 100CPM, 3° Strain, 12 minutes by RPA-2000
 3.0 dNmMin S', 150°C, 100CPM, 3° Strain, 12 minutes by RPA-2000
Volume Change (%)0.1Aniline, 40°C, after 168 hr, Suitable
 0.1Diethylene glycol, 40°C, after 168 hr, Suitable
 0.1Diethylene glycol, 40°C, after 500 hr, Suitable
 0.2Ethylene glycol, 40°C, after 168 hr, Suitable
 0.3Ethylene glycol, 40°C, after 500 hr, Suitable
 0.3Isophorone, 25°C, after 168 hr, Suitable
 0.3Aniline, 40°C, after 500 hr, Suitable
 0.3Sulfuric acid 96%, 40°C, after 168 hr, Suitable
 0.3Sodium hydroxide 48%, 40°C, after 168 hr, Suitable
 0.3Sodium hypochlorite 5%, 40°C, after 168 hr, Suitable
 0.3Formalin 35%, 40°C, after 168 hr, Suitable
 0.4Sodium hypochlorite 5%, 40°C, after 500 hr, Suitable
 0.4Isophorone, 25°C, after 500 hr, Suitable
 0.5Acetophenone, 40°C, after 168 hr, Suitable
 0.5Sulfuric acid 96%, 40°C, after 500 hr, Suitable
 0.5Dimethyl acetamide, 40°C, after 168 hr, Suitable
 0.5N-Methyl-2-pyrrolidone, 40°C, after 168 hr, Suitable
 0.6Dimethyl formamide, 40°C, after 168 hr, Suitable
 0.6N-Methyl-2-pyrrolidone, 40°C, after 500 hr, Suitable
 0.6Formalin 35%, 40°C, after 500 hr, Suitable
 0.7Ethanol, 40°C, after 168 hr, Suitable
 0.8Acetophenone, 40°C, after 500 hr, Suitable
 0.8Dioxane, 40°C, after 168 hr, Suitable
 0.8Dimethyl acetamide, 40°C, after 500 hr, Suitable
 0.8ASTM Oil No.1, 175°C, after 168 hr, Suitable
 0.9Gear Oil, 175°C, after 168 hr, Suitable
 0.9Dimethyl formamide, 40°C, after 500 hr, Suitable
 0.9Nitric acid 60%, 40°C, after 168 hr, Suitable
 0.9Hydrochloric acid 35%, 40°C, after 168 hr, Suitable
 1Gear Oil, 175°C, after 500 hr, Suitable
 1ASTM Oil No.1, 175°C, after 500 hr, Suitable
 1Aqueous ammonia 28%, 40°C, after 168 hr, Suitable
 1Hydrochloric acid 35%, 40°C, after 500 hr, Suitable
 1.1Methanol, 40°C, after 168 hr, Suitable
 1.1Engine oil (SJ), 175°C, after 168 hr, Suitable
 1.1Ethanol, 40°C, after 500 hr, Suitable
 1.2Engine oil (SJ), 175°C, after 500 hr, Suitable
 1.3Methyl isobutyl ketone, 40°C, after 168 hr, Suitable
 1.4Dioxane, 40°C, after 500 hr, Suitable
 1.4Formic acid 88%, 40°C, after 168 hr, Suitable
 1.4Sodium hydroxide 48%, 40°C, after 500 hr, Suitable
 1.4Nitric acid 60%, 40°C, after 500 hr, Suitable
 1.5ATF, 175°C, after 168 hr, Suitable
 1.6Ethylene diamine, 40°C, after 168 hr, Suitable
 1.6Aqueous ammonia 28%, 40°C, after 500 hr, Suitable
 1.7ATF, 175°C, after 500 hr, Suitable
 1.7Xylene, 40°C, after 168 hr, Suitable
 1.7Methanol, 40°C, after 500 hr, Suitable
 1.8Acetylacetone, 40°C, after 168 hr, Suitable
 1.9Butyl acetate, 40°C, after 168 hr, Suitable
 1.9Isooctane, 40°C, after 168 hr, Suitable
 2Cyclohexane, 40°C, after 168 hr, Suitable
 2Methyl isobutyl ketone, 40°C, after 500 hr, Suitable
 2.1Acetaldehyde, 25°C, after 168 hr, Suitable
 2.3Formic acid 88%, 40°C, after 500 hr, Suitable
 2.3Acetic anhydride, 40°C, after 168 hr, Suitable
 2.4dichloromethane, 25°C, after 168 hr, Suitable
 2.5Acetylacetone, 40°C, after 500 hr, Suitable
 2.5Toluene, 40°C, after 168 hr, Suitable
 2.5ASTM Oil No.3, 175°C, after 500 hr, Suitable
 2.6Xylene, 40°C, after 500 hr, Suitable
 2.6ASTM Oil No.3, 175°C, after 168 hr, Suitable
 2.8Butyl acetate, 40°C, after 500 hr, Suitable
 2.8Acetaldehyde, 25°C, after 500 hr, Suitable
 2.9Acetone, 40°C, after 168 hr, Suitable
 2.9Methyl ethyl ketone, 40°C, after 168 hr, Suitable
 3Cyclohexane, 40°C, after 500 hr, Suitable
 3.1Isooctane, 40°C, after 500 hr, Suitable
 3.1Diethyl ether, 25°C, after 168 hr, Suitable
 3.4Benzene, 40°C, after 168 hr, Suitable
 3.52-Methyltetrahydrofuran, 40°C, after 168 hr, Suitable
 3.5Acetone, 40°C, after 500 hr, Suitable
 3.5Methyl ethyl ketone, 40°C, after 500 hr, Suitable
 3.6Tetrachloroethylene, 40°C, after 168 hr, Suitable
 3.6Toluene, 40°C, after 500 hr, Suitable
 3.6dichloromethane, 25°C, after 500 hr, Suitable
 3.7Acetic anhydride, 40°C, after 500 hr, Suitable
 3.7Ethyl acetate, 40°C, after 168 hr, Suitable
 3.9Tetrahydrofuran 35%, 40°C, after 168 hr, Suitable
 4.2Ethyl acetate, 40°C, after 500 hr, Suitable
 4.3Ethylene diamine, 40°C, after 500 hr, Suitable
 4.4Benzene, 40°C, after 500 hr, Suitable
 4.5Steam, 170°C, after 168 hr, Suitable
 4.5Steam, 170°C, after 500 hr, Suitable
 4.6Hexane, 40°C, after 168 hr, Suitable
 4.9Diethyl ether, 25°C, after 500 hr, Suitable
 5Tetrachloroethylene, 40°C, after 500 hr, Applicable
 5.1Tetrahydrofuran 35%, 40°C, after 500 hr, Applicable
 5.22-Methyltetrahydrofuran, 40°C, after 500 hr, Applicable
 5.5Hexane, 40°C, after 500 hr, Applicable
 5.5Carbon tetrachloride, 40°C, after 168 hr, Applicable
 5.8Trichloroethylene, 40°C, after 168 hr, Applicable
 6.1Trichloroethylene, 40°C, after 500 hr, Applicable
 6.4Chloroform, 40°C, after 168 hr, Applicable
 6.9Chloroform, 40°C, after 500 hr, Applicable
 8.5Carbon tetrachloride, 40°C, 500 hr 168 hr, Applicable

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
AGC AFLAS® PM-3000 TFE/P Perfluoroelastomer
AGC AFLAS® 150P TFE/P Fluoroelastomers
AGC AFLAS® 100H TFE/P Fluoroelastomers
AGC AFLAS® 100S TFE/P Fluoroelastomers
AGC AFLAS® 150C TFE/P Fluoroelastomers

PAGCX001 / 191110

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.