MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Specialty Compounds RTP Company

Mitsui Milastomer™ 5030NS Natural Vulcanized Thermoplastic Elastomer
Categories: Polymer; Thermoplastic; Elastomer, TPE; Thermoplastic Vulcanizate Elastomer (TPV)

Material Notes: General Purpose Grade.

Information provided by Mitsui.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.880 g/cc0.0318 lb/in³ASTM D1505
Melt Flow 30 g/10 min
@Load 10.0 kg,
Temperature 230 °C
30 g/10 min
@Load 22.0 lb,
Temperature 446 °F
ISO 1133
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A  48
@Time 5.00 sec
48
@Time 0.00139 hour
ISO 48
 51
@Time 0.000 sec
51
@Time 0.000 hour
ISO 48
Tensile Strength at Break 3.40 MPa493 psiJIS No. 3 Dumbbell; 500 mm/min.; ISO 37
Elongation at Break 540 %540 %JIS No. 3 Dumbbell; 500 mm/min.; ISO 37
100% Modulus 1.20 MPa
@Strain 100 %
174 psi
@Strain 100 %
JIS No. 3 Dumbbell; 500 mm/min.; ISO 37
Compression Set  26 %
@Temperature 23.0 °C,
Time 79200 sec
26 %
@Temperature 73.4 °F,
Time 22.0 hour
ISO 815
 44 %
@Temperature 70.0 °C,
Time 79200 sec
44 %
@Temperature 158 °F,
Time 22.0 hour
ISO 815
 
Thermal PropertiesMetricEnglishComments
Brittleness Temperature <= -60.0 °C<= -76.0 °F
 
Descriptive Properties
Major UsesGrip, Compound
ProcessingInjection Molding

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Alliance Polymers Viprene™ G45A-32U-BLK Thermoplastic Vulcanizate Elastomer
Top Polymer Topolymer® 9210-403 Thermoplastic Vulcanized Elastomer
Teknor Apex Sarlink® TPV 22035N Thermoplastic Vulcanizate
Ravago Manufacturing Americas EZPrene 9040A TPV
ExxonMobil Santoprene® 8191-55B100 Thermoplastic Elastomer

PMIT9934 / 222963

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.