MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger PEI

APCM DA 4518 Epoxy Pregpreg System
Categories: Polymer; Thermoset; Epoxy

Material Notes: Description: DA 4518 is an epoxy prepreg designed for a temperature range of -67°F (-55°C) to 350°F (177°C), with a cure of 250°F (121°C) for one hour and or a cure of 350º F (177ºC) for 1 hour. This material needs to be post cure or cured to 350ºF to get the 350º properties

Mechanical Properties: The data supplied are averages obtained on 12 plies of DA 4518 on 7781 glass cured one hour at 250°F (121°C) with a heat up rate of 5° per minute from room temperature.

Information provided by Adhesive Prepegs for Composite Manufacturers, LLC

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Volatiles <= 1.0 %<= 1.0 %
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength  476 MPa
@Temperature 82.2 °C
69000 psi
@Temperature 180 °F
ASTM D638
 496 MPa
@Temperature 23.9 °C
72000 psi
@Temperature 75.0 °F
ASTM D638
Tensile Modulus  29.6 GPa
@Temperature 23.9 °C
4300 ksi
@Temperature 75.0 °F
ASTM D638
 31.0 GPa
@Temperature 82.2 °C
4500 ksi
@Temperature 180 °F
ASTM D638
Flexural Strength  290 MPa
@Temperature 177 °C
42000 psi
@Temperature 350 °F
ASTM D790
 758 MPa
@Temperature 82.2 °C
110000 psi
@Temperature 180 °F
ASTM D790
 786 MPa
@Temperature 23.9 °C
114000 psi
@Temperature 75.0 °F
ASTM D790
 290 MPa
@Temperature 177 °C,
Time 86400 sec
42000 psi
@Temperature 350 °F,
Time 24.0 hour
ASTM D790
Flexural Modulus  31.7 GPa
@Temperature 23.9 °C
4600 ksi
@Temperature 75.0 °F
ASTM D790
 31.7 GPa
@Temperature 82.2 °C
4600 ksi
@Temperature 180 °F
ASTM D790
 
Processing PropertiesMetricEnglishComments
Cure Time 60.0 min
@Temperature 121 °C
1.00 hour
@Temperature 250 °F
Gel Time 10.0 min
@Temperature 121 °C
10.0 min
@Temperature 250 °F
Shelf Life  1.00 Month
@Temperature 23.9 °C
1.00 Month
@Temperature 75.0 °F
 6.00 Month
@Temperature 4.44 °C
6.00 Month
@Temperature 40.0 °F
 12.0 Month
@Temperature -17.8 °C
12.0 Month
@Temperature 0.000 °F
 
Descriptive Properties
FormModified epoxy impregnated fabric
Resin Content45-50%
SeparatorRelease paper and poly film

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Solvay CYCOM® 934 Epoxy - E-Glass Fiber Reinforced Unidirectional Tape and Roving Laminate
Solvay CYCOM® 5216 Epoxy - Unidirectional S-Glass Prepreg, After Environmental Exposure
Solvay CYCOM® 5216 Epoxy - Unidirectional S-Glass Prepreg
Solvay CYCOM® 5216 Epoxy - Unidirectional E-Glass Prepreg, After Environmental Exposure
Solvay CYCOM® 5216 Epoxy - Unidirectional E-Glass Prepreg

PAPCM006 / 187019

Visit Zeus Inc. for PEEK Tubing

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.