MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

(Viewing data as-entered. Click here to return)
Haynes Hastelloy® G-35® Nickel Alloy Gas Tungsten Arc Welded (GTAW) Plate
Categories: Metal; Nonferrous Metal; Nickel Alloy

Material Notes: Known for its corrosion performance, HASTELLOY® G-35® alloy was designed to resist “wet process” phosphoric acid, which is widely used in the production of fertilizers. Tests indicate that it is far superior to HASTELLOY® G-30® alloy and stainless steels, in this chemical. It was also designed to resist localized attack in the presence of chlorides, since under-deposit attack is a potential problem in evaporators used to concentrate “wet process” phosphoric acid. As a result of its high-chromium content, G-35 alloy is extremely resistant to other oxidizing acids, such as nitric, and mixtures containing nitric acid. It possesses moderate resistance to reducing acids, as a result of its appreciable molybdenum content, and, unlike other nickel-chromium-molybdenum alloys, it is very resistant to “caustic dealloying” in hot sodium hydroxide. Finally, G-35 alloy is much less susceptible to chloride-induced stress corrosion cracking than the high chromium stainless steels and nickel-chromium-iron alloys traditionally used in “wet process” phosphoric acid.

G-35 alloy is available in the form of plate, sheet, strip, billet, bar, wire, covered electrodes, pipe, and tubing.

Potential Applications:

  • “Wet process” phosphoric acid evaporators.
  • Pickling in nitric and hydrofluoric acids.
  • Chemical process industry systems involving nitric and chlorides.
  • Caustic neutralizing systems.
  • Systems requiring resistance to high temperature corrosion at 800-1200°F.

G-35 alloy is covered by ASME, ASTM, and DIN specifications.

Welding: The weldability of G-35 alloy is similar to that of C-276 alloy. To weld G-35 alloy, three processes are commonly used. For sheet welds and plate root passes, gas tungsten arc (GTAW) welding is favored. For plate welds, the gas metal arc (GMAW) process is preferred. For field welding, the shielded metal arc process, using coated electrodes, is favored. Submerged arc welding is not recommended as this process is characterized by high heat input to the base metal and slow cooling of the weld. To minimize the precipitation of second phases in regions affected by the heat of welding, a maximum interpass temperature of 93°C (200°F) is recommended for G-35 alloy. Also, welding of cold-worked materials is strongly discouraged, since they sensitize more quickly and induce residual stresses. A full solution anneal, followed by water quenching, is recommended for cold-worked structures, prior to welding.

Joining Base Metal Preparation: The joint surface and adjacent area should be thoroughly cleaned before welding. All grease, oil crayon marks, sulfur compounds, and other foreign matter should be removed.

Filler Metal Selections: For gas tungsten arc and gas metal arc welding, G-35 filler wire is suggested. For shielded metal arc welding, G-35 covered electrodes are suggested.

Heat Treatment: Wrought forms of HASTELLOY G-35 alloy are furnished in the solution annealed condition, unless otherwise specified. The standard solution annealing treatment consists of heating to 1121°C (2050°F) followed by rapid air-cooling or water quenching. Parts which have been hot formed should be solution annealed prior to final fabrication or installation.

Forming: G-35 alloy has excellent forming characteristics, and cold forming is the preferred method of shaping. The alloy can be easily cold worked due to its good ductility. The alloy is generally stiffer than the austenitic stainless steels; therefore, more energy is required during cold forming.

Tensile properties reported are for transverse gas tungsten arc welded plate specimens. Other properties are typical of the alloy.

Data provided by the manufacturer, Haynes International, Inc.

Vendors: Visit metalmen for your metals needs. Products include special chemistry, tight tolerances, custom tempers, odd dimensions/forms, and small quantities. Phone 1-800-767-9494.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Density 8.22 g/cc
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength, Ultimate 448 MPa
@Thickness 12.7 mm,
Temperature 538 °C
 545 MPa
@Thickness 12.7 mm,
Temperature 260 °C
 696 MPa
@Thickness 12.7 mm,
Temperature 25.0 °C
Tensile Strength, Yield 249 MPa
@Thickness 12.7 mm,
Temperature 538 °C
0.2% Offset
 310 MPa
@Thickness 12.7 mm,
Temperature 260 °C
0.2% Offset
 438 MPa
@Thickness 12.7 mm,
Temperature 25.0 °C
0.2% Offset
Elongation at Break 37 %
@Thickness 12.7 mm,
Temperature 538 °C
 40 %
@Thickness 12.7 mm,
Temperature 260 °C
 44 %
@Thickness 12.7 mm,
Temperature 25.0 °C
Modulus of Elasticity 170 GPa
@Temperature 649 °C
Dynamic
 177 GPa
@Temperature 538 °C
Dynamic
 183 GPa
@Temperature 427 °C
Dynamic
 189 GPa
@Temperature 316 °C
Dynamic
 204 GPa
@Temperature 25.0 °C
Dynamic
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.000118 ohm-cm
@Temperature 25.0 °C
 0.000119 ohm-cm
@Temperature 100 °C
 0.000120 ohm-cm
@Temperature 200 °C
 0.000121 ohm-cm
@Temperature 300 °C
 0.000122 ohm-cm
@Temperature 400 °C
 0.000124 ohm-cm
@Temperature 500 °C
 0.000125 ohm-cm
@Temperature 600 °C
 
Thermal PropertiesOriginal ValueComments
CTE, linear 12.3 µm/m-°C
@Temperature 21.0 - 100 °C
 12.6 µm/m-°C
@Temperature 21.0 - 200 °C
 13.2 µm/m-°C
@Temperature 21.0 - 300 °C
 13.4 µm/m-°C
@Temperature 21.0 - 400 °C
 13.6 µm/m-°C
@Temperature 21.0 - 500 °C
 14.4 µm/m-°C
@Temperature 21.0 - 600 °C
Specific Heat Capacity 0.450 J/g-°C
@Temperature 25.0 °C
 0.470 J/g-°C
@Temperature 100 °C
 0.490 J/g-°C
@Temperature 200 °C
 0.510 J/g-°C
@Temperature 300 °C
 0.530 J/g-°C
@Temperature 400 °C
 0.530 J/g-°C
@Temperature 500 °C
 0.600 J/g-°C
@Temperature 600 °C
Thermal Conductivity 10.0 W/m-K
@Temperature 25.0 °C
 12.0 W/m-K
@Temperature 100 °C
 14.0 W/m-K
@Temperature 200 °C
 16.0 W/m-K
@Temperature 300 °C
 18.0 W/m-K
@Temperature 400 °C
 19.0 W/m-K
@Temperature 500 °C
 23.0 W/m-K
@Temperature 600 °C
Melting Point 1332 - 1361 °C
Solidus 1332 °C
Liquidus 1361 °C
 
Processing PropertiesOriginal ValueComments
Annealing Temperature 2050 °FFollowed by rapid air cooling or water quench
 
Component Elements PropertiesOriginal ValueComments
Aluminum, Al <= 0.40 %
Carbon, C <= 0.050 %
Chromium, Cr 33 %
Iron, Fe <= 2.0 %
Manganese, Mn <= 0.50 %
Molybdenum, Mo 8.0 %
Nickel, Ni 55.5 %as balance
Silicon, Si <= 0.60 %
 
Descriptive Properties
Thermal Diffusivity0.028 cm2/s25°C
 0.031 cm2/s100°C
 0.034 cm2/s200°C
 0.038 cm2/s300°C
 0.042 cm2/s400°C
 0.045 cm2/s500°C
 0.048 cm2/s600°C

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Haynes Hastelloy® G-30® alloy, 9.5 mm thick plate
Haynes Hastelloy® G-35® Nickel Alloy Sheet, Annealed at 2075°F (1135°C)
Carpenter Invar 36® Alloy, Cold Drawn Bars
MetalTek MTEK CW-12MW Cast UNS N30002 Severe Corrosion and Heat Resistant Alloy
MetalTek MTEK CW-2M Cast UNS N26455 Severe Corrosion and Heat Resistant Alloy

NHAY975 / 162642

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.