MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Specialty Compounds RTP Company

Covestro Texin® 255 Thermoplastic Polyurethanes (TPU) (Extended Aging Data)
Categories: Polymer; Thermoplastic; Polyurethane, TP

Material Notes: Texin 255 resin is a polyester-based thermoplastic polyurethane with a Shore hardness of approximately 55D. It can be processed by injection molding; extrusion processes are not recommended.

Properties / Applications: Texin 255 natural color resin complies with FDA food-contact regulations 21 CFR 177.1680 (Polyurethane Resins) and 177.2600 (Rubber Articles Intended for Repeated Use), for use in articles that contact food except articles used for packing or holding food during cooking, subject to the limitations of these and any other applicable regulations. Texin 255 resin offers excellent fuel and oil resistance, as well as outstanding abrasion resistance, impact strength, toughness, and flexibility. Typical applications include toplifts, seals, gaskets, sleeves, casters, and gears.

Information provided by Covestro

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.21 g/cc1.21 g/ccASTM D792
Linear Mold Shrinkage, Flow 0.0080 cm/cm
@Thickness 2.54 mm
0.0080 in/in
@Thickness 0.100 in
ASTM D955
Linear Mold Shrinkage, Transverse 0.0080 cm/cm
@Thickness 2.54 mm
0.0080 in/in
@Thickness 0.100 in
ASTM D955
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore D 5555ASTM D2240
 47
@Temperature 504 °C
47
@Temperature 939 °F
Fuel C; ASTM D471
 48
@Temperature 70.0 °C
48
@Temperature 158 °F
Fuel C; ASTM D471
 49
@Temperature 336 °C
49
@Temperature 637 °F
Fuel C; ASTM D471
 51
@Temperature 70.0 °C
51
@Temperature 158 °F
Fuel A; ASTM D471
 51
@Temperature 168 °C
51
@Temperature 334 °F
Fuel C; ASTM D471
 54
@Temperature 336 °C
54
@Temperature 637 °F
Fuel A; ASTM D471
 56
@Temperature 168 °C
56
@Temperature 334 °F
Fuel A; ASTM D471
 60
@Temperature 504 °C
60
@Temperature 939 °F
Fuel A; ASTM D471
 50
@Treatment Temp. 336 °C,
Time 125 sec
50
@Treatment Temp. 637 °F,
Time 0.0347 hour
Hot Air; ASTM D573
 51
@Treatment Temp. 504 °C,
Time 125 sec
51
@Treatment Temp. 939 °F,
Time 0.0347 hour
Hot Air; ASTM D573
 53
@Treatment Temp. 70.0 °C,
Time 100 sec
53
@Treatment Temp. 158 °F,
Time 0.0278 hour
Hot Air; ASTM D573
 53
@Treatment Temp. 336 °C,
Time 100 sec
53
@Treatment Temp. 637 °F,
Time 0.0278 hour
ASTM Oil #1; ASTM D471
 54
@Treatment Temp. 168 °C,
Time 100 sec
54
@Treatment Temp. 334 °F,
Time 0.0278 hour
Hot Air; ASTM D573
 54
@Treatment Temp. 504 °C,
Time 100 sec
54
@Treatment Temp. 939 °F,
Time 0.0278 hour
ASTM Oil #3; ASTM D471
 55
@Treatment Temp. 168 °C,
Time 125 sec
55
@Treatment Temp. 334 °F,
Time 0.0347 hour
Hot Air; ASTM D573
 55
@Treatment Temp. 336 °C,
Time 100 sec
55
@Treatment Temp. 637 °F,
Time 0.0278 hour
Hot Air; ASTM D573
 55
@Treatment Temp. 504 °C,
Time 100 sec
55
@Treatment Temp. 939 °F,
Time 0.0278 hour
Hot Air; ASTM D573
 55
@Treatment Temp. 504 °C,
Time 100 sec
55
@Treatment Temp. 939 °F,
Time 0.0278 hour
ASTM Oil #1; ASTM D471
 56
@Treatment Temp. 168 °C,
Time 100 sec
56
@Treatment Temp. 334 °F,
Time 0.0278 hour
ASTM Oil #1; ASTM D471
 56
@Treatment Temp. 70.0 °C,
Time 125 sec
56
@Treatment Temp. 158 °F,
Time 0.0347 hour
Hot Air; ASTM D573
 57
@Treatment Temp. 70.0 °C,
Time 100 sec
57
@Treatment Temp. 158 °F,
Time 0.0278 hour
ASTM Oil #1; ASTM D471
 57
@Treatment Temp. 70.0 °C,
Time 100 sec
57
@Treatment Temp. 158 °F,
Time 0.0278 hour
ASTM Oil #3; ASTM D471
Tensile Strength at Break 63.4 MPa9200 psiASTM D412
 56.426 MPa
@Time 1.81e+6 sec
8183.9 psi
@Time 504 hour
Fuel C; ASTM D471
 57.06 MPa
@Time 1.21e+6 sec
8276 psi
@Time 336 hour
Fuel C; ASTM D471
 60.864 MPa
@Time 605000 sec
8827.6 psi
@Time 168 hour
Fuel C; ASTM D471
 61.498 MPa
@Time 605000 sec
8919.5 psi
@Time 168 hour
Fuel A; ASTM D471
 62.766 MPa
@Time 1.81e+6 sec
9103.5 psi
@Time 504 hour
Fuel A; ASTM D471
 64.034 MPa
@Time 252000 sec
9287.4 psi
@Time 70.0 hour
Fuel C; ASTM D471
 67.204 MPa
@Time 1.21e+6 sec
9747.1 psi
@Time 336 hour
Fuel A; ASTM D471
 67.204 MPa
@Time 252000 sec
9747.1 psi
@Time 70.0 hour
Fuel A; ASTM D471
 45.014 MPa
@Treatment Temp. 100 °C,
Time 1.81e+6 sec
6528.7 psi
@Treatment Temp. 212 °F,
Time 504 hour
ASTM Oil #1; ASTM D471
 46.282 MPa
@Treatment Temp. 125 °C,
Time 1.81e+6 sec
6712.6 psi
@Treatment Temp. 257 °F,
Time 504 hour
Hot Air; ASTM D573
 48.818 MPa
@Treatment Temp. 125 °C,
Time 1.21e+6 sec
7080.5 psi
@Treatment Temp. 257 °F,
Time 336 hour
Hot Air; ASTM D573
 50.72 MPa
@Treatment Temp. 100 °C,
Time 1.21e+6 sec
7356 psi
@Treatment Temp. 212 °F,
Time 336 hour
ASTM Oil #1; ASTM D471
 50.72 MPa
@Treatment Temp. 125 °C,
Time 252000 sec
7356 psi
@Treatment Temp. 257 °F,
Time 70.0 hour
Hot Air; ASTM D573
 51.988 MPa
@Treatment Temp. 100 °C,
Time 1.81e+6 sec
7540.2 psi
@Treatment Temp. 212 °F,
Time 504 hour
ASTM Oil #3; ASTM D471
 56.426 MPa
@Treatment Temp. 125 °C,
Time 605000 sec
8183.9 psi
@Treatment Temp. 257 °F,
Time 168 hour
Hot Air; ASTM D573
 60.864 MPa
@Treatment Temp. 100 °C,
Time 605000 sec
8827.6 psi
@Treatment Temp. 212 °F,
Time 168 hour
ASTM Oil #1; ASTM D471
 65.302 MPa
@Treatment Temp. 100 °C,
Time 252000 sec
9471.3 psi
@Treatment Temp. 212 °F,
Time 70.0 hour
Hot Air; ASTM D573
 68.472 MPa
@Treatment Temp. 100 °C,
Time 605000 sec
9931.0 psi
@Treatment Temp. 212 °F,
Time 168 hour
Hot Air; ASTM D573
 72.16 MPa
@Treatment Temp. 100 °C,
Time 1.21e+6 sec
10470 psi
@Treatment Temp. 212 °F,
Time 336 hour
Hot Air; ASTM D573
 72.16 MPa
@Treatment Temp. 100 °C,
Time 1.81e+6 sec
10470 psi
@Treatment Temp. 212 °F,
Time 504 hour
Hot Air; ASTM D573
 74.812 MPa
@Treatment Temp. 100 °C,
Time 252000 sec
10851 psi
@Treatment Temp. 212 °F,
Time 70.0 hour
ASTM Oil #1; ASTM D471
 75.446 MPa
@Treatment Temp. 100 °C,
Time 252000 sec
10943 psi
@Treatment Temp. 212 °F,
Time 70.0 hour
ASTM Oil #3; ASTM D471
Tensile Stress at Strain  12.4 MPa
@Strain 50 %
1800 psi
@Strain 50 %
ASTM D412
 15.9 MPa
@Strain 100 %
2310 psi
@Strain 100 %
ASTM D412
 32.4 MPa
@Strain 300 %
4700 psi
@Strain 300 %
ASTM D412
 15.59 MPa
@Strain 100 %,
Temperature 125 °C
2261 psi
@Strain 100 %,
Temperature 257 °F
Hot Air, 168; ASTM D412
 16.218 MPa
@Strain 100 %,
Temperature 100 °C
2352.2 psi
@Strain 100 %,
Temperature 212 °F
ASTM Oil #3, 504; ASTM D471
 16.536 MPa
@Strain 100 %,
Temperature 100 °C
2398.3 psi
@Strain 100 %,
Temperature 212 °F
Hot Air, 168; ASTM D573
 16.536 MPa
@Strain 100 %,
Temperature 125 °C
2398.3 psi
@Strain 100 %,
Temperature 257 °F
Hot Air, 504; ASTM D573
 17.013 MPa
@Strain 100 %,
Temperature 125 °C
2467.5 psi
@Strain 100 %,
Temperature 257 °F
Hot Air, 70; ASTM D412
 17.172 MPa
@Strain 100 %,
Temperature 125 °C
2490.6 psi
@Strain 100 %,
Temperature 257 °F
Hot Air, 336; ASTM D573
 17.649 MPa
@Strain 100 %,
Temperature 100 °C
2559.8 psi
@Strain 100 %,
Temperature 212 °F
Hot Air, 70; ASTM D573
 17.808 MPa
@Strain 100 %,
Temperature 100 °C
2582.8 psi
@Strain 100 %,
Temperature 212 °F
ASTM Oil #1, 70; ASTM D573
 17.967 MPa
@Strain 100 %,
Temperature 100 °C
2605.9 psi
@Strain 100 %,
Temperature 212 °F
Hot Air, 336; ASTM D573
 18.126 MPa
@Strain 100 %,
Temperature 100 °C
2629.0 psi
@Strain 100 %,
Temperature 212 °F
Hot Air, 504; ASTM D573
 18.126 MPa
@Strain 100 %,
Temperature 100 °C
2629.0 psi
@Strain 100 %,
Temperature 212 °F
ASTM Oil #1, 168; ASTM D573
 18.126 MPa
@Strain 100 %,
Temperature 100 °C
2629.0 psi
@Strain 100 %,
Temperature 212 °F
ASTM Oil #1, 336; ASTM D471
 18.285 MPa
@Strain 100 %,
Temperature 100 °C
2652.0 psi
@Strain 100 %,
Temperature 212 °F
ASTM Oil #1, 50; ASTM D471
 18.444 MPa
@Strain 100 %,
Temperature 100 °C
2675.1 psi
@Strain 100 %,
Temperature 212 °F
ASTM Oil #3, 70; ASTM D471
 22.68 MPa
@Strain 100 %,
Temperature 125 °C
3289 psi
@Strain 100 %,
Temperature 257 °F
Hot Air, 504; ASTM D471
 23.652 MPa
@Strain 100 %,
Temperature 125 °C
3430.4 psi
@Strain 100 %,
Temperature 257 °F
Hot Air, 336; ASTM D471
 24.948 MPa
@Strain 100 %,
Temperature 125 °C
3618.4 psi
@Strain 100 %,
Temperature 257 °F
Hot Air, 70; ASTM D471
 27.54 MPa
@Strain 100 %,
Temperature 125 °C
3994 psi
@Strain 100 %,
Temperature 257 °F
Hot Air, 168; ASTM D471
 27.864 MPa
@Strain 300 %,
Temperature 100 °C
4041.3 psi
@Strain 300 %,
Temperature 212 °F
ASTM Oil #1, 50; ASTM D471
 28.512 MPa
@Strain 300 %,
Temperature 100 °C
4135.3 psi
@Strain 300 %,
Temperature 212 °F
ASTM Oil #3, 504; ASTM D471
 29.484 MPa
@Strain 300 %,
Temperature 100 °C
4276.3 psi
@Strain 300 %,
Temperature 212 °F
ASTM Oil #1, 336; ASTM D471
 30.78 MPa
@Strain 300 %,
Temperature 100 °C
4464 psi
@Strain 300 %,
Temperature 212 °F
Hot Air, 168; ASTM D573
 32.076 MPa
@Strain 300 %,
Temperature 100 °C
4652.2 psi
@Strain 300 %,
Temperature 212 °F
Hot Air, 336; ASTM D573
 32.724 MPa
@Strain 300 %,
Temperature 100 °C
4746.2 psi
@Strain 300 %,
Temperature 212 °F
Hot Air, 70; ASTM D573
 32.724 MPa
@Strain 300 %,
Temperature 100 °C
4746.2 psi
@Strain 300 %,
Temperature 212 °F
Hot Air, 504; ASTM D573
 33.048 MPa
@Strain 300 %,
Temperature 100 °C
4793.2 psi
@Strain 300 %,
Temperature 212 °F
ASTM Oil #1, 168; ASTM D471
 34.668 MPa
@Strain 300 %,
Temperature 100 °C
5028.2 psi
@Strain 300 %,
Temperature 212 °F
ASTM Oil #1, 70; ASTM D471
 36.612 MPa
@Strain 300 %,
Temperature 100 °C
5310.1 psi
@Strain 300 %,
Temperature 212 °F
ASTM Oil #3, 336; ASTM D471
 10.812 MPa
@Strain 300 %,
Time 1.21e+6 sec
1568.2 psi
@Strain 300 %,
Time 336 hour
Fuel C; ASTM D471
 11.607 MPa
@Time 605000 sec,
Strain 300 %
1683.5 psi
@Time 168 hour,
Strain 300 %
Fuel C; ASTM D471
 11.607 MPa
@Strain 300 %,
Time 1.81e+6 sec
1683.5 psi
@Strain 300 %,
Time 504 hour
Fuel C; ASTM D471
 12.879 MPa
@Time 252000 sec,
Strain 300 %
1867.9 psi
@Time 70.0 hour,
Strain 300 %
Fuel C; ASTM D471
 15.582 MPa
@Time 605000 sec,
Strain 300 %
2260.0 psi
@Time 168 hour,
Strain 300 %
Fuel A; ASTM D471
 16.218 MPa
@Time 252000 sec,
Strain 300 %
2352.2 psi
@Time 70.0 hour,
Strain 300 %
Fuel A; ASTM D471
 16.377 MPa
@Strain 300 %,
Time 1.21e+6 sec
2375.3 psi
@Strain 300 %,
Time 336 hour
Fuel A; ASTM D471
 16.695 MPa
@Strain 300 %,
Time 1.81e+6 sec
2421.4 psi
@Strain 300 %,
Time 504 hour
Fuel A; ASTM D471
 21.06 MPa
@Strain 100 %,
Time 1.21e+6 sec
3055 psi
@Strain 100 %,
Time 336 hour
Fuel C; ASTM D471
 21.384 MPa
@Strain 100 %,
Time 605000 sec
3101.5 psi
@Strain 100 %,
Time 168 hour
Fuel C; ASTM D471
 23.628 MPa
@Strain 100 %,
Time 1.81e+6 sec
3427.0 psi
@Strain 100 %,
Time 504 hour
Fuel C; ASTM D471
 25.272 MPa
@Time 252000 sec,
Strain 100 %
3665.4 psi
@Time 70.0 hour,
Strain 100 %
Fuel C; ASTM D471
 28.836 MPa
@Strain 100 %,
Time 605000 sec
4182.3 psi
@Strain 100 %,
Time 168 hour
Fuel A; ASTM D471
 32.076 MPa
@Strain 100 %,
Time 1.21e+6 sec
4652.2 psi
@Strain 100 %,
Time 336 hour
Fuel A; ASTM D471
 33.372 MPa
@Strain 100 %,
Time 1.81e+6 sec
4840.2 psi
@Strain 100 %,
Time 504 hour
Fuel A; ASTM D471
 34.02 MPa
@Time 252000 sec,
Strain 100 %
4934 psi
@Time 70.0 hour,
Strain 100 %
Fuel A; ASTM D471
Elongation at Break 500 %500 %ASTM D412
 460 %
@Time 1.81e+6 sec
460 %
@Time 504 hour
Fuel C; ASTM D471
 480 %
@Time 1.21e+6 sec
480 %
@Time 336 hour
Fuel A; ASTM D471
 480 %
@Time 252000 sec
480 %
@Time 70.0 hour
Fuel A; ASTM D471
 490 %
@Time 1.21e+6 sec
490 %
@Time 336 hour
Fuel C; ASTM D471
 490 %
@Time 1.81e+6 sec
490 %
@Time 504 hour
Fuel A; ASTM D471
 525 %
@Time 252000 sec
525 %
@Time 70.0 hour
Fuel C; ASTM D471
 530 %
@Time 605000 sec
530 %
@Time 168 hour
Fuel C; ASTM D471
 545 %
@Time 605000 sec
545 %
@Time 168 hour
Fuel A; ASTM D471
 485 %
@Treatment Temp. 100 °C,
Time 252000 sec
485 %
@Treatment Temp. 212 °F,
Time 70.0 hour
Hot Air; ASTM D573
 530 %
@Treatment Temp. 100 °C,
Time 252000 sec
530 %
@Treatment Temp. 212 °F,
Time 70.0 hour
ASTM Oil #3; ASTM D471
 535 %
@Treatment Temp. 100 °C,
Time 605000 sec
535 %
@Treatment Temp. 212 °F,
Time 168 hour
Hot Air; ASTM D573
 540 %
@Treatment Temp. 100 °C,
Time 252000 sec
540 %
@Treatment Temp. 212 °F,
Time 70.0 hour
ASTM Oil #1; ASTM D471
 560 %
@Treatment Temp. 100 °C,
Time 605000 sec
560 %
@Treatment Temp. 212 °F,
Time 168 hour
ASTM Oil #1; ASTM D471
 570 %
@Treatment Temp. 100 °C,
Time 1.21e+6 sec
570 %
@Treatment Temp. 212 °F,
Time 336 hour
Hot Air; ASTM D573
 575 %
@Treatment Temp. 100 °C,
Time 1.81e+6 sec
575 %
@Treatment Temp. 212 °F,
Time 504 hour
Hot Air; ASTM D573
 580 %
@Treatment Temp. 100 °C,
Time 1.81e+6 sec
580 %
@Treatment Temp. 212 °F,
Time 504 hour
ASTM Oil #1; ASTM D471
 600 %
@Treatment Temp. 100 °C,
Time 1.81e+6 sec
600 %
@Treatment Temp. 212 °F,
Time 504 hour
ASTM Oil #3; ASTM D471
 620 %
@Treatment Temp. 125 °C,
Time 605000 sec
620 %
@Treatment Temp. 257 °F,
Time 168 hour
Hot Air; ASTM D573
 620 %
@Treatment Temp. 100 °C,
Time 1.21e+6 sec
620 %
@Treatment Temp. 212 °F,
Time 336 hour
ASTM Oil #1; ASTM D471
 640 %
@Treatment Temp. 125 °C,
Time 252000 sec
640 %
@Treatment Temp. 257 °F,
Time 70.0 hour
Hot Air; ASTM D573
 650 %
@Treatment Temp. 125 °C,
Time 1.81e+6 sec
650 %
@Treatment Temp. 257 °F,
Time 504 hour
Hot Air; ASTM D573
 675 %
@Treatment Temp. 125 °C,
Time 1.21e+6 sec
675 %
@Treatment Temp. 257 °F,
Time 336 hour
Hot Air; ASTM D573
Flexural Modulus  0.0517 GPa
@Temperature 70.0 °C
7.50 ksi
@Temperature 158 °F
ASTM D790
 0.0689 GPa
@Temperature 23.0 °C
9.99 ksi
@Temperature 73.4 °F
ASTM D790
 1.207 GPa
@Temperature -30.0 °C
175.1 ksi
@Temperature -22.0 °F
ASTM D790
Compressive Strength 1.00 MPa145 psi2% Deflection; ASTM D 575
 3.90 MPa566 psi5% Deflection; ASTM D 575
 7.40 MPa1070 psi10% Deflection; ASTM D 575
 10.1 MPa1460 psi15% Deflection; ASTM D 575
 12.7 MPa1840 psi20% Deflection; ASTM D 575
 15.5 MPa2250 psi25% Deflection; ASTM D 575
 40.6 MPa5890 psi50% Deflection; ASTM D 575
Resilience 4040[%], Bayshore; ASTM D2632
Shear Strength 38.51 MPa5585 psiASTM D732
Dart Drop, Total Energy  50.0 J
@Thickness 2.54 mm,
Temperature -30.0 °C
36.9 ft-lb
@Thickness 0.100 in,
Temperature -22.0 °F
5 ph, 3-in clamp; ASTM D3763
 57.8 J
@Thickness 2.54 mm,
Temperature 23.0 °C
42.6 ft-lb
@Thickness 0.100 in,
Temperature 73.4 °F
5 ph, 3-in clamp; ASTM D3763
Tear Strength 157.6 kN/m899.3 pliDie C; ASTM D624
Taber Abrasion, mg/1000 Cycles 50
@Load 1.00 kg
50
@Load 2.20 lb
[mg] Loss, H-18; ASTM D3489
Compression Set  15 %
@Temperature 23.0 °C,
Time 79200 sec
15 %
@Temperature 73.4 °F,
Time 22.0 hour
postcured; ASTM D395-B
 20 %
@Temperature 23.0 °C,
Time 79200 sec
20 %
@Temperature 73.4 °F,
Time 22.0 hour
as molded; ASTM D395-B
 35 %
@Temperature 70.0 °C,
Time 79200 sec
35 %
@Temperature 158 °F,
Time 22.0 hour
postcured; ASTM D395-B
 50 %
@Temperature 100 °C,
Time 79200 sec
50 %
@Temperature 212 °F,
Time 22.0 hour
postcured; ASTM D395-B
 65 %
@Temperature 70.0 °C,
Time 79200 sec
65 %
@Temperature 158 °F,
Time 22.0 hour
as molded; ASTM D395-B
 75 %
@Temperature 100 °C,
Time 79200 sec
75 %
@Temperature 212 °F,
Time 22.0 hour
as molded; ASTM D395-B
 
Thermal PropertiesMetricEnglishComments
CTE, linear 131 µm/m-°C73.0 µin/in-°FASTM D696
Deflection Temperature at 0.46 MPa (66 psi) 59.0 °C138 °FASTM D648
Vicat Softening Point 138 °C280 °FRate A; ASTM D1525
Brittleness Temperature >= -55.6 °C>= -68.0 °FASTM D746
Glass Transition Temp, Tg -26.0 °C-14.8 °F
Flammability, UL94 HB
@Thickness 1.50 mm
HB
@Thickness 0.0591 in
 
Processing PropertiesMetricEnglishComments
Rear Barrel Temperature 193 - 210 °C379 - 410 °F
Middle Barrel Temperature 193 - 216 °C379 - 421 °F
Front Barrel Temperature 199 - 221 °C390 - 430 °F
Nozzle Temperature 204 - 227 °C399 - 441 °F
Melt Temperature 210 °C410 °F
Mold Temperature 15.0 - 40.0 °C59.0 - 104 °F
Injection Pressure 41.4 - 103 MPa6000 - 15000 psi
 
Compliance PropertiesMetricEnglishComments
FDA YesYes

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Covestro Texin® 255 Thermoplastic Polyurethanes (TPU)

PCOVEST0976a / 238175

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.