MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Haynes Hastelloy® S alloy, flat products, solution heat-treated at 649°C (1200°F), aged 8000 hours
Categories: Metal; Nonferrous Metal; Nickel Alloy; Superalloy

Material Notes: Nickel-based, high temperature alloy. Excellent thermal stability, low thermal expansion, excellent oxidation resistance to 1093°C, good high temperature and thermal fatigue strength. Applications include seal rings in gas turbine engines, and severe cyclical heating conditions where it retains strength, ductility, and integrity.

Data provided by the manufacturer, Haynes International, Inc.

Key Words: UNS N06635, AMS 5711, AMS 5838, AMS 5873
Vendors: Visit metalmen for your metals needs. Products include special chemistry, tight tolerances, custom tempers, odd dimensions/forms, and small quantities. Phone 1-800-767-9494.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Density 8.75 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell A 56
@Thickness 12.7 mm
 56
@Thickness 1.45 mm
Tensile Strength, Ultimate 877 MPa
@Thickness 12.7 mm
 914 MPa
@Thickness 1.45 mm
Tensile Strength, Yield 393 MPa
@Strain 0.2 %,
Thickness 12.7 mm
 454 MPa
@Strain 0.2 %,
Thickness 1.45 mm
Elongation at Break 50 %
@Thickness 12.7 mm
in 50.8 mm
 54 %
@Thickness 1.45 mm
in 50.8 mm
Modulus of Elasticity 132 GPa
@Temperature 1093 °C
Heat treated at 1066°C, air cooled
 151 GPa
@Temperature 927 °C
Heat treated at 1066°C, air cooled
 161 GPa
@Temperature 813 °C
Heat treated at 1066°C, air cooled
 166 GPa
@Temperature 760 °C
Heat treated at 1066°C, air cooled
 174 GPa
@Temperature 649 °C
Heat treated at 1066°C, air cooled
 182 GPa
@Temperature 538 °C
Heat treated at 1066°C, air cooled
 194 GPa
@Temperature 357 °C
Heat treated at 1066°C, air cooled
 212 GPa
@Temperature 24.0 °C
Charpy Impact 190 JV Notch; plate
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.000128 ohm-cm
@Temperature 25.0 °C
specimen aged 16000 hours at 650°C (1200°F)
 
Thermal PropertiesOriginal ValueComments
CTE, linear 11.5 µm/m-°C
@Temperature 20.0 - 93.0 °C
 12.2 µm/m-°C
@Temperature 20.0 - 204 °C
 12.8 µm/m-°C
@Temperature 20.0 - 316 °C
 13.1 µm/m-°C
@Temperature 20.0 - 427 °C
 13.3 µm/m-°C
@Temperature 20.0 - 538 °C
 14.4 µm/m-°C
@Temperature 20.0 - 760 °C
 14.9 µm/m-°C
@Temperature 20.0 - 871 °C
 15.5 µm/m-°C
@Temperature 20.0 - 982 °C
 16.0 µm/m-°C
@Temperature 20.0 - 1093 °C
Specific Heat Capacity 0.398 J/g-°C
@Temperature 0.000 °C
 0.414 J/g-°C
@Temperature 50.0 °C
 0.440 J/g-°C
@Temperature 150 °C
 0.456 J/g-°C
@Temperature 250 °C
 0.473 J/g-°C
@Temperature 350 °C
 0.481 J/g-°C
@Temperature 450 °C
 0.494 J/g-°C
@Temperature 550 °C
 0.502 J/g-°C
@Temperature 650 °C
 0.590 J/g-°C
@Temperature 800 °C
 0.594 J/g-°C
@Temperature 850 °C
 0.594 J/g-°C
@Temperature 900 °C
 0.594 J/g-°C
@Temperature 700 °C
 0.594 J/g-°C
@Temperature 750 °C
 0.598 J/g-°C
@Temperature 950 °C
 0.598 J/g-°C
@Temperature 1000 °C
 0.598 J/g-°C
@Temperature 1050 °C
 0.603 J/g-°C
@Temperature 1100 °C
Thermal Conductivity 14.0 W/m-K
@Temperature 200 °C
 16.1 W/m-K
@Temperature 300 °C
 17.9 W/m-K
@Temperature 400 °C
 19.5 W/m-K
@Temperature 500 °C
 21.0 W/m-K
@Temperature 600 °C
 26.1 W/m-K
@Temperature 700 °C
 26.1 W/m-K
@Temperature 800 °C
 26.1 W/m-K
@Temperature 900 °C
 27.1 W/m-K
@Temperature 950 °C
 28.0 W/m-K
@Temperature 1000 °C
Melting Point 1335 - 1380 °C
Solidus 1335 °C
Liquidus 1380 °C
Maximum Service Temperature, Air 1093 °C
 
Component Elements PropertiesOriginal ValueComments
Aluminum, Al 0.10 - 0.50 %
Boron, B <= 0.015 %
Carbon, C <= 0.020 %
Chromium, Cr 14.5 - 17 %
Cobalt, Co <= 2.0 %
Copper, Cu <= 0.35 %
Iron, Fe <= 3.0 %
Lanthanum, La 0.010 - 0.10 %
Manganese, Mn 0.30 - 1.0 %
Molybdenum, Mo 14 - 16.5 %
Nickel, Ni 67 %
Phosphorus, P <= 0.020 %
Silicon, Si 0.20 - 0.75 %
Sulfur, S <= 0.015 %
Tungsten, W <= 1.0 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
ATI Allvac® Nickelvac® H-X Nickel Superalloy, Heat Treatment: 1177°C (2150°F) Anneal
Haynes Hastelloy® D-205 Corrosion Resistant Alloy
Haynes Hastelloy® N, 1.6 mm sheet, heat treated at 1175°C, rapid air cooled
Haynes Hastelloy® S alloy, flat products, solution heat-treated at 649°C (1200°F), aged 1000 hours
Latitude Manufacturing PowderFlo® X Metal Injection Molding Compound

NHASAZ / 16904

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.