MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
Eastman Tenite 285A3R30018 Butyrate Natural, Trsp  (discontinued **)
Categories: Polymer; Renewable/Recycled Polymer; Thermoplastic; Cellulosic; Cellulose Acetate Butyrate, Molded

Material Notes: Tenite cellulosic plastics are noted for their excellent balance of properties - toughness, hardness, strength, surface gloss, clarity, and a warm feel. The mechanical properties of Tenite cellulosic plastics differ with plasticizer levels. Lower plasticizer content yields a harder surface, higher heat resistance, greater rigidity, higher tensile strength, and better dimensional stability. Higher plasticizer content increases impact strength. Tenite cellulose plastics are available in natural, clear, selected ambers, or smoke transparents and black translucents. Color concentrates are available in let-down ratios from 10:1 to 40:1. Tenite Cellulose Acetate Butyrate 285-18 has a plasticizer level of 18% and contains an odor mask.

Applications/Uses

  • Ophthalmic
  • Optical safety frames
  • Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
     
    Physical PropertiesOriginal ValueComments
    Specific Gravity 1.17 g/ccASTM D792
    Water Absorption 1.3 %24h Immersion; ASTM D570
    Collected Volatile Condensable Material 0.90 %Weight loss on heating, 72hrs, 80°C; ASTM D707
     
    Mechanical PropertiesOriginal ValueComments
    Hardness, Rockwell R 26ASTM D785
    Tensile Strength at Break 30.7 MPaASTM D638
    Tensile Strength, Yield 23.5 MPaASTM D638
    Elongation at Break 50 %ASTM D638
    Flexural Yield Strength 30.4 MPaASTM D790
    Flexural Modulus 1.034 GPaASTM D790
    Izod Impact, Notched 1.10 J/cm
    @Temperature -40.0 °C
    ASTM D256
     358 J/m
    @Temperature 23.0 °C
    ASTM D256
     
    Thermal PropertiesOriginal ValueComments
    Deflection Temperature at 0.46 MPa (66 psi) 75.0 °CASTM D648
    Deflection Temperature at 1.8 MPa (264 psi) 61.0 °CASTM D648
    Vicat Softening Point 94.0 °CASTM D1525
     
    Optical PropertiesOriginal ValueComments
    Haze <= 8.5 %ASTM D1003
     
    Descriptive Properties
    Plasticizer, %18
    Soluble Matter Loss, %0.1ASTM D570

    **
    Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

    Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

    Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

    Users viewing this material also viewed the following:
    Eastman Tenite Butyrate 575E3720010 Clear, Trsp Cellulose Acetate Butyrate

    PE9100 / 35156

    Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

    The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.