MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

SACO AEI THERMODAN® HF TP343NT Low Smoke Zero Halogen Jacket Compound
Categories: Polymer; Thermoplastic

Material Notes: Description: THERMODAN® HF TP343NT is a Patent Pending High Performance, Low Smoke Halogen-Free, Thermoplastic Wire and Cable Compound. This compound has superior fire performance, low smoke production and contains no halogens. When used as a jacket for Fiber Optic Cables, TP343NT can assist the cable maker in meeting the stringent new European CPR Regulations at the B2ca Classification (Cable Design Dependant | Actual Results May Vary). THERMODAN® HF TP343NT is natural in color, UV resistant, and is certified Halogen Free by UL to UL2885

High Performance Characteristics | Technology Advantages

  • High Performance Characteristics: Flame Spread | Total Heat Release | Fire Growth Rate | Low Smoke | Flaming Droplets | Low Acidity (European Standard EN 50575)
  • Capable of VW-1 performance applied at 30 mils on 14 AWG copper conductor
  • Wide Processing Window | Low Die Drool
High Performance Markets:
  • Recommended for Fiber Optic Cable Jackets 2-24 Fiber Carriers
  • Fiber optic cable LSZH jacket capable to meet European CPR B2ca classification (Cable Design Dependant | Actual Results May Vary)
  • High Performance Markets: Hospitals | Airports | Commercial Premises & Residential Facilities

Information provided by SACO AEI Polymers.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.64 g/cc1.64 g/ccASTM D792
pH 5.785.78combustion Gas; IEC 60754-2
Melt Flow 18 g/10 min
@Load 21.6 kg,
Temperature 190 °C
18 g/10 min
@Load 47.6 lb,
Temperature 374 °F
ASTM D1238
Storage Temperature <= 29.4 °C<= 85.0 °F
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A 96
@Time 1.00 sec
96
@Time 0.000278 hour
ASTM D2240
Tensile Strength at Break 10.3 MPa1500 psiUL 2556
 >= 7.757 MPa
@Temperature 70.0 °C,
Time 14400 sec
>= 1125 psi
@Temperature 158 °F,
Time 4.00 hour
Oil; UL 2556
 >= 8.791 MPa
@Temperature 113 °C,
Time 605000 sec
>= 1275 psi
@Temperature 235 °F,
Time 168 hour
after thermal ageing; UL 2556
 >= 8.791 MPa
@Temperature 121 °C,
Time 605000 sec
>= 1275 psi
@Temperature 250 °F,
Time 168 hour
after thermal ageing; UL 2556
 >= 8.27 MPa
@Time 2.59e+6 sec
>= 1200 psi
@Time 720 hour
Weather-o-meter; UL 2556
Elongation at Break 200 %200 %UL 2556
 >= 140 %
@Temperature 113 °C,
Time 605000 sec
>= 140 %
@Temperature 235 °F,
Time 168 hour
after thermal ageing; UL 2556
 >= 140 %
@Temperature 121 °C,
Time 605000 sec
>= 140 %
@Temperature 250 °F,
Time 168 hour
after thermal ageing; UL 2556
 >= 180 %
@Temperature 70.0 °C,
Time 14400 sec
>= 180 %
@Temperature 158 °F,
Time 4.00 hour
Oil; UL 2556
 >= 160 %
@Time 2.59e+6 sec
>= 160 %
@Time 720 hour
Weather-o-meter; UL 2556
Flexural Modulus, 1% Secant 131 MPa19000 psiASTM D790
 
Electrical PropertiesMetricEnglishComments
Dielectric Constant  3.88
@Frequency 1e+6 Hz
3.88
@Frequency 1e+6 Hz
ASTM D2520
 3.94
@Frequency 3.50e+8 Hz
3.94
@Frequency 3.50e+8 Hz
ASTM D2520
 3.94
@Frequency 5.00e+8 Hz
3.94
@Frequency 5.00e+8 Hz
ASTM D2520
 3.94
@Frequency 6.00e+8 Hz
3.94
@Frequency 6.00e+8 Hz
ASTM D2520
 3.94
@Frequency 1e+9 Hz
3.94
@Frequency 1e+9 Hz
ASTM D2520
 3.98
@Frequency 1000 Hz
3.98
@Frequency 1000 Hz
ASTM D2520
Dissipation Factor  0.0055
@Frequency 1e+9 Hz
0.0055
@Frequency 1e+9 Hz
ASTM D150
 0.0060
@Frequency 6.00e+8 Hz
0.0060
@Frequency 6.00e+8 Hz
ASTM D150
 0.0065
@Frequency 5.00e+8 Hz
0.0065
@Frequency 5.00e+8 Hz
ASTM D150
 0.0069
@Frequency 3.50e+8 Hz
0.0069
@Frequency 3.50e+8 Hz
ASTM D150
 0.0117
@Frequency 1000 Hz
0.0117
@Frequency 1000 Hz
ASTM D150
 0.0207
@Frequency 1e+6 Hz
0.0207
@Frequency 1e+6 Hz
ASTM D150
 
Thermal PropertiesMetricEnglishComments
Brittleness Temperature -39.0 °C-38.2 °F3 min in methanol; ASTM D638
Smoke Density 188188Flaming, corrected; ASTM E662
 221221Non-flaming, corrected; ASTM E662
 3.0
@Time 240 sec
3.0
@Time 0.0667 hour
Non-flaming; ASTM E662
 5.0
@Time 240 sec
5.0
@Time 0.0667 hour
Flaming; ASTM E662
Oxygen Index 38 %38 %ASTM D2863
 
Processing PropertiesMetricEnglishComments
Processing Temperature 135 - 171 °C275 - 340 °Fbarrel zones
Die Temperature 179 °C354 °F
Head Temperature 177 °C351 °F
 
Descriptive Properties
Conductivity0.243 µS/mmof Gasses, IEC 60754-2

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PSACO011 / 249378

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.