MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Morgan Advanced Ceramics Firelite 124-G Thermal Ceramic
Categories: Ceramic; Oxide

Material Notes: Insulating Aggregate raw material base. Hydraulic bond. Insulating castable for service up to 1100°C/2010°F. It has exceptional strength in relation to low density and low thermal conductivity. Can be used in applications similar to those described by UOP 2-18-0. Conforms to classes O and P of ASTM classification C-401-84.

Information provided by Morgan Advanced Materials

Key Words: Thermal Ceramics
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Bulk Density 1.06 g/cc0.0383 lb/in³dried to 110°C
Grain Size <= 8000 µm<= 8000 µm
 
Mechanical PropertiesMetricEnglishComments
Compressive Strength  2.50 MPa
@Treatment Temp. 1000 °C
363 psi
@Treatment Temp. 1830 °F
Cold Crushing Strength
 4.20 MPa
@Treatment Temp. 815 °C
609 psi
@Treatment Temp. 1500 °F
Cold Crushing Strength
 5.90 MPa
@Treatment Temp. 110 °C
856 psi
@Treatment Temp. 230 °F
Cold Crushing Strength
 
Thermal PropertiesMetricEnglishComments
Thermal Conductivity  0.200 W/m-K
@Temperature 200 °C
1.39 BTU-in/hr-ft²-°F
@Temperature 392 °F
ASTM C 417
 0.210 W/m-K
@Temperature 400 °C
1.46 BTU-in/hr-ft²-°F
@Temperature 752 °F
ASTM C 417
 0.240 W/m-K
@Temperature 600 °C
1.67 BTU-in/hr-ft²-°F
@Temperature 1110 °F
ASTM C 417
Maximum Service Temperature, Air <= 1100 °C<= 2010 °F
Shrinkage 0.60 %0.60 %MST
 0.20 %
@Treatment Temp. 815 °C
0.20 %
@Treatment Temp. 1500 °F
 0.30 %
@Treatment Temp. 1000 °C
0.30 %
@Treatment Temp. 1830 °F
 
Component Elements PropertiesMetricEnglishComments
Al2O3 31.5 %31.5 %
CaO 22 %22 %
Fe2O3 9.6 %9.6 %
K2O+Na2O 3.3 %3.3 %Na2O+ K2O
SiO2 30 %30 %
TiO2 1.4 %1.4 %
 
Descriptive Properties
Net Material Required (kg/m³)920
Water Addition50% by weight, 25kg bag weight

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Morgan Advanced Ceramics Firelite 124 Thermal Ceramic

CMORF6257 / 203041

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.