MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

RheTech Products G20P100-01 20% Glass Fiber Reinforced Polypropylene, Black
Categories: Polymer; Thermoplastic; Polypropylene (PP); Polypropylene with 20% Glass Fiber Filler

Material Notes: Applications:
  • Arm rest insert
  • Vacuum canister
  • Storage bin
  • Consoles
  • Battery trays

Injection molding conditions reported in table.

Information provided by RheTech Products.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.05 g/cc
@Temperature 23.0 °C
1.05 g/cc
@Temperature 73.4 °F
23/23°C; ASTM D792
Filler Content 20 %20 %ASTM D5630
Linear Mold Shrinkage 0.0028 cm/cm0.0028 in/inASTM D955
Melt Flow 5.0 g/10 min
@Load 2.16 kg,
Temperature 230 °C
5.0 g/10 min
@Load 4.76 lb,
Temperature 446 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore D 7272ASTM D2240
Tensile Strength at Break 64.1 MPa9300 psi2 in/min; ASTM D638
Flexural Modulus 3.59 GPa520 ksiTangent; ASTM D790
Izod Impact, Notched 0.641 J/cm
@Temperature 23.0 °C
1.20 ft-lb/in
@Temperature 73.4 °F
ASTM D256
Gardner Impact 0.678 J0.500 ft-lbASTM D5420
 
Thermal PropertiesMetricEnglishComments
Deflection Temperature at 0.46 MPa (66 psi) 157 °C314 °FASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 139 °C282 °FASTM D648
 
Processing PropertiesMetricEnglishComments
Rear Barrel Temperature 199 - 227 °C390 - 440 °F
Middle Barrel Temperature 204 - 232 °C400 - 450 °F
Front Barrel Temperature 210 - 238 °C410 - 460 °F
Nozzle Temperature 216 - 227 °C420 - 440 °F
Mold Temperature 26.7 - 48.9 °C80.0 - 120 °F
Drying Temperature 65.6 - 82.2 °C150 - 180 °F
Dry Time 1 - 2 hour1 - 2 hour
Moisture Content <= 0.050 %<= 0.050 %Recommended
Injection Pressure 2.76 - 10.3 MPa400 - 1500 psi
Hold Pressure 2.07 - 8.27 MPa300 - 1200 psi
Back Pressure 0.345 - 1.03 MPa50.0 - 150 psi

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
RheTech Products GC20P100-01 20% Glass Fiber Reinforced Polypropylene, Chemically Coupled, Black
Phillips Sumika Marlex® AMN-010 Polypropylene Impact Copolymer
Asahi Kasei Thermylene® P6-20FG-0753 20% Glass Fiber Reinforced, Heat Stabilized Polypropylene
RheTech Products T20P100-01 20% Talc Reinforced Polypropylene, Black
LyondellBasell Pro-fax SV152 Polypropylene Impact Copolymer

PRHET145 / 65713

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.