MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

Corning Eagle XG® Slim Display Glass
Categories: Ceramic; Glass; Optical

Material Notes: Alkaline earth boro-aluminosilicate fusion drawn sheet glass used for active matrix flat panel displays

Information provided by Corning Incorporated.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 2.38 g/cc0.0860 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Vickers 640640kg(f)/mm² (200 g load; 25 s dwell)
Modulus of Elasticity 73.6 GPa10700 ksi
Poissons Ratio 0.230.23
Shear Modulus 30.1 GPa4370 ksi
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity  6.30e+8 ohm-cm
@Temperature 500 °C
6.30e+8 ohm-cm
@Temperature 932 °F
 7.90e+12 ohm-cm
@Temperature 250 °C
7.90e+12 ohm-cm
@Temperature 482 °F
Dielectric Constant  5.3
@Frequency 200 - 100000 Hz,
Temperature 23.0 °C
5.3
@Frequency 200 - 100000 Hz,
Temperature 73.4 °F
 5.4
@Frequency 200 - 100000 Hz,
Temperature 200 °C
5.4
@Frequency 200 - 100000 Hz,
Temperature 392 °F
 5.4
@Frequency 10000 - 100000 Hz,
Temperature 300 °C
5.4
@Frequency 10000 - 100000 Hz,
Temperature 572 °F
 5.5
@Frequency 1000 Hz,
Temperature 300 °C
5.5
@Frequency 1000 Hz,
Temperature 572 °F
 5.5
@Frequency 100000 Hz,
Temperature 400 °C
5.5
@Frequency 100000 Hz,
Temperature 752 °F
 5.6
@Frequency 10000 Hz,
Temperature 400 °C
5.6
@Frequency 10000 Hz,
Temperature 752 °F
 5.6
@Frequency 100000 Hz,
Temperature 500 °C
5.6
@Frequency 100000 Hz,
Temperature 932 °F
 5.6
@Frequency 200 Hz,
Temperature 300 °C
5.6
@Frequency 200 Hz,
Temperature 572 °F
 5.9
@Frequency 1000 Hz,
Temperature 400 °C
5.9
@Frequency 1000 Hz,
Temperature 752 °F
 6.0
@Frequency 10000 Hz,
Temperature 500 °C
6.0
@Frequency 10000 Hz,
Temperature 932 °F
 6.3
@Frequency 200 Hz,
Temperature 400 °C
6.3
@Frequency 200 Hz,
Temperature 752 °F
 7.2
@Frequency 1000 Hz,
Temperature 500 °C
7.2
@Frequency 1000 Hz,
Temperature 932 °F
 8.2
@Frequency 200 Hz,
Temperature 500 °C
8.2
@Frequency 200 Hz,
Temperature 932 °F
Dissipation Factor  0.0010
@Frequency 200 - 10000 Hz,
Temperature 23.0 °C
0.0010
@Frequency 200 - 10000 Hz,
Temperature 73.4 °F
 0.0010
@Frequency 200 - 10000 Hz,
Temperature 125 °C
0.0010
@Frequency 200 - 10000 Hz,
Temperature 257 °F
 0.0011
@Frequency 10000 Hz,
Temperature 200 °C
0.0011
@Frequency 10000 Hz,
Temperature 392 °F
 0.0012
@Frequency 1000 Hz,
Temperature 200 °C
0.0012
@Frequency 1000 Hz,
Temperature 392 °F
 0.0013
@Frequency 200 Hz,
Temperature 200 °C
0.0013
@Frequency 200 Hz,
Temperature 392 °F
 0.010
@Frequency 100000 Hz,
Temperature 400 °C
0.010
@Frequency 100000 Hz,
Temperature 752 °F
 0.013
@Frequency 10000 Hz,
Temperature 400 °C
0.013
@Frequency 10000 Hz,
Temperature 752 °F
 0.11
@Frequency 1000 Hz,
Temperature 400 °C
0.11
@Frequency 1000 Hz,
Temperature 752 °F
 0.13
@Frequency 200 Hz,
Temperature 400 °C
0.13
@Frequency 200 Hz,
Temperature 752 °F
 
Thermal PropertiesMetricEnglishComments
CTE, linear  3.17 µm/m-°C
@Temperature 0.000 - 300 °C
1.76 µin/in-°F
@Temperature 32.0 - 572 °F
 3.55 µm/m-°C
@Temperature 25.0 - 675 °C
1.97 µin/in-°F
@Temperature 77.0 - 1250 °F
Specific Heat Capacity  0.768 J/g-°C
@Temperature 23.0 °C
0.184 BTU/lb-°F
@Temperature 73.4 °F
 0.896 J/g-°C
@Temperature 100 °C
0.214 BTU/lb-°F
@Temperature 212 °F
 0.998 J/g-°C
@Temperature 200 °C
0.239 BTU/lb-°F
@Temperature 392 °F
 1.067 J/g-°C
@Temperature 300 °C
0.2550 BTU/lb-°F
@Temperature 572 °F
 1.11 J/g-°C
@Temperature 400 °C
0.265 BTU/lb-°F
@Temperature 752 °F
 1.154 J/g-°C
@Temperature 500 °C
0.2758 BTU/lb-°F
@Temperature 932 °F
Thermal Conductivity  >= 1.09 W/m-K
@Temperature 23.0 °C
>= 7.56 BTU-in/hr-ft²-°F
@Temperature 73.4 °F
 >= 1.22 W/m-K
@Temperature 100 °C
>= 8.47 BTU-in/hr-ft²-°F
@Temperature 212 °F
 >= 1.29 W/m-K
@Temperature 200 °C
>= 8.95 BTU-in/hr-ft²-°F
@Temperature 392 °F
 >= 1.34 W/m-K
@Temperature 300 °C
>= 9.30 BTU-in/hr-ft²-°F
@Temperature 572 °F
 >= 1.37 W/m-K
@Temperature 400 °C
>= 9.51 BTU-in/hr-ft²-°F
@Temperature 752 °F
 >= 1.42 W/m-K
@Temperature 500 °C
>= 9.85 BTU-in/hr-ft²-°F
@Temperature 932 °F
Softening Point 971 °C1780 °F107.6 Poise
Working Point 1293 °C2359 °F104 Poise
Annealing Point 722 °C1330 °F1013 Poise
Strain Point 669 °C1240 °F1014.5 Poise
 
Optical PropertiesMetricEnglishComments
Refractive Index  1.5078
@Wavelength 643.8 nm
1.5078
@Wavelength 643.8 nm
 1.5099
@Wavelength 589.3 nm
1.5099
@Wavelength 589.3 nm
 1.5119
@Wavelength 546.1 nm
1.5119
@Wavelength 546.1 nm
 1.5141
@Wavelength 508.6 nm
1.5141
@Wavelength 508.6 nm
 1.516
@Wavelength 480 nm
1.516
@Wavelength 480 nm
 1.5169
@Wavelength 467.8 nm
1.5169
@Wavelength 467.8 nm
 1.5198
@Wavelength 435.8 nm
1.5198
@Wavelength 435.8 nm
Transmission, Visible 90 %
@Wavelength 375 - 800 nm,
Thickness 0.400 mm
90 %
@Wavelength 375 - 800 nm,
Thickness 0.0157 in
IR Transmittance  91.1 %
@Wavelength 1200 nm
91.1 %
@Wavelength 1200 nm
 91.9 %
@Wavelength 1750 nm
91.9 %
@Wavelength 1750 nm
 92.2 %
@Wavelength 2000 nm
92.2 %
@Wavelength 2000 nm
UV Transmittance  0.00 %
@Wavelength 200 - 250 nm,
Thickness 0.400 mm
0.00 %
@Wavelength 200 - 250 nm,
Thickness 0.0157 in
 40 %
@Thickness 0.400 mm,
Wavelength 300 nm
40 %
@Thickness 0.0157 in,
Wavelength 300 nm
 80 %
@Thickness 0.400 mm,
Wavelength 340 nm
80 %
@Thickness 0.0157 in,
Wavelength 340 nm
 90 %
@Thickness 0.400 mm,
Wavelength 375 nm
90 %
@Thickness 0.0157 in,
Wavelength 375 nm
 
Descriptive Properties
Birefringence Constant331 (nm/cm)/(kg/mm²)

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Schott D 263 Thin Borosilicate Glass
Solvay Thornel® T-650/42 12K Carbon Fiber, Polyacrylonitrile (PAN) Precursor
Poco Graphite SUPERSiC® Basic Silicon Carbide
SGL Carbon Group EK 20 Carbon Graphite
Solvay Thornel® T-650/35 3K Carbon Fiber, Polyacrylonitrile (PAN) Precursor

CCORNG992 / 197398

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.