MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Refractory Metals

(Viewing data as-entered. Click here to return)
Tantalum, Ta; Sintered, Cast (UNS R05210)
Categories: Metal; Nonferrous Metal; Refractory Metal; Pure Element

Material Notes: Sintered unalloyed

Characteristics: high corrosion resistance, fine microstructure, excellent cold ductility, excellent formability and weldability

Key Words: UNS R05210
Vendors: Eagle Alloys Corporation is a leading supplier of quality metals and alloys. Our staff prides itself on working fast, efficiently and courteously to get you the information you need. Call (800) 237-9012 or visit www.EagleAlloys.com.

PLANSEE SE: Whether it's high temperatures, aggressive chemicals or extreme mechanical loading: PLANSEE supplies a suitable product solution in refractory metals or composite materials. As the world market leader in powder metallurgically produced high performance materials we combine outstanding materials knowledge with profound applications and technology know-how. Visit us at www.plansee.com.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Density 16.656 g/cc
a Lattice Constant 3.303 Åbody-centered cubic
Vapor Pressure 5.00e-13 bar
@Temperature 1800 °C
 7.00e-10 bar
@Temperature 2200 °C
 
Chemical PropertiesOriginal ValueComments
Atomic Mass 180.95
Atomic Number 73
Atomic Volume 1.8e-029m^3
 
Mechanical PropertiesOriginal ValueComments
Hardness, Vickers 120
Tensile Strength, Ultimate 310 MPa
Tensile Strength, Yield 220 MPa
@Strain 0.2 %
Elongation at Break 30 %
Modulus of Elasticity 185 GPa
 150 GPa
@Temperature 1200 °C
 155 GPa
@Temperature 800 °C
 165 GPa
@Temperature 400 °C
Poissons Ratio 0.35
Shear Modulus 68.5 GPaCalculated
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.0000125 ohm-cm
 
Thermal PropertiesOriginal ValueComments
CTE, linear 6.50 µm/m-°C
 6.70 µm/m-°C
@Temperature 200 °C
 6.90 µm/m-°C
@Temperature 600 °C
 7.10 µm/m-°C
@Temperature 1000 °C
Specific Heat Capacity 0.139 J/g-°C
 0.140 J/g-°C
@Temperature 400 °C
 0.150 J/g-°C
@Temperature 800 °C
 0.170 J/g-°C
@Temperature 1200 °C
Thermal Conductivity 57.55 W/m-K
 53.0 W/m-K
@Temperature 200 °C
 55.0 W/m-K
@Temperature 400 °C
 57.0 W/m-K
@Temperature 600 °C
Melting Point 2996 °C
Boiling Point 5460 °C
 
Processing PropertiesOriginal ValueComments
Recrystallization Temperature 900 - 1450 °CAnnealing time: 1 hour
 
Component Elements PropertiesOriginal ValueComments
Tantalum, Ta 100 %impurities not specified

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
H.C. Starck NRC® Tantalum (UNS R05200)
Tantalum, UNS R05400
Tantalum, Ta; Annealed
CeramTec ATZ Alumina Toughened Zirconia, Dental Grade
Tantalum, UNS R05200

MRTa01 / 100351

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.