MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Specialty Compounds RTP Company

Toray AMILAN™ CM1001G-20 Nylon 6, 20% Glass Fiber
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 6 (PA6); Nylon 6, 20% Glass Fiber Filled

Material Notes: Reinforced, high flow, PA6-GF20.

General Amilan™ Notes: AMILAN™ nylon (polyamide) is a thermoplastic engineering plastic containing an amide group (-CONH-) and it exhibits excellent strength, toughness, heat resistance, and anti-friction wear resistance. A variety of grades designed for various customer needs and applications are available.

Information provided by Toray Resin Co.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.29 g/cc0.0466 lb/in³Dry; ISO 1183
Water Absorption 7.8 %7.8 %In 23°C water, polymer initally dry; ISO 62
 1.3 %
@Time 86400 sec
1.3 %
@Time 24.0 hour
In 23°C water, polymer initally dry; ISO 62
Linear Mold Shrinkage, Flow 0.0030 - 0.0050 cm/cm0.0030 - 0.0050 in/in80x80x3mmt. Dry; Toray Method
 0.0060 - 0.0090 cm/cm0.0060 - 0.0090 in/in80x80x3mmt. Dry; Toray Method
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell M 9292Dry; ISO 2039-2
Hardness, Rockwell R  12
@Temperature 80.0 °C
12
@Temperature 176 °F
Dry; ISO 2039-2
 120
@Temperature 23.0 °C
120
@Temperature 73.4 °F
Dry; ISO 2039-2
Tensile Strength 120 MPa
@Temperature 23.0 °C
17400 psi
@Temperature 73.4 °F
Dry; ISO 527-1,2
Elongation at Break  2.5 %
@Temperature -40.0 °C
2.5 %
@Temperature -40.0 °F
Dry; ISO 527-1,2
 3.0 %
@Temperature 23.0 °C
3.0 %
@Temperature 73.4 °F
Dry; ISO 527-1,2
 3.0 %
@Temperature -40.0 °C
3.0 %
@Temperature -40.0 °F
3.0% Moisture Content; ISO 527-1,2
 4.5 %
@Temperature 23.0 °C
4.5 %
@Temperature 73.4 °F
3.0% Moisture Content; ISO 527-1,2
 5.0 %
@Temperature 80.0 °C
5.0 %
@Temperature 176 °F
Dry; ISO 527-1,2
 5.5 %
@Temperature 80.0 °C
5.5 %
@Temperature 176 °F
3.0% Moisture Content; ISO 527-1,2
Flexural Strength  115 MPa
@Temperature 80.0 °C
16700 psi
@Temperature 176 °F
Dry; ISO 178
 205 MPa
@Temperature 23.0 °C
29700 psi
@Temperature 73.4 °F
Dry; ISO 178
 275 MPa
@Temperature -40.0 °C
39900 psi
@Temperature -40.0 °F
Dry; ISO 178
Flexural Modulus  2.60 GPa
@Temperature 80.0 °C
377 ksi
@Temperature 176 °F
3.0% Moisture Content; ISO 178
 3.20 GPa
@Temperature 80.0 °C
464 ksi
@Temperature 176 °F
Dry; ISO 178
 3.50 GPa
@Temperature 23.0 °C
508 ksi
@Temperature 73.4 °F
3.0% Moisture Content; ISO 178
 6.80 GPa
@Temperature 23.0 °C
986 ksi
@Temperature 73.4 °F
Dry; ISO 178
 7.30 GPa
@Temperature -40.0 °C
1060 ksi
@Temperature -40.0 °F
3.0% Moisture Content; ISO 178
 8.70 GPa
@Temperature -40.0 °C
1260 ksi
@Temperature -40.0 °F
Dry; ISO 178
Compressive Strength  80.0 MPa
@Temperature 23.0 °C
11600 psi
@Temperature 73.4 °F
3.0% Moisture Content; ISO 604
 90.0 MPa
@Temperature 80.0 °C
13100 psi
@Temperature 176 °F
Dry; ISO 604
 155 MPa
@Temperature 23.0 °C
22500 psi
@Temperature 73.4 °F
Dry; ISO 604
 240 MPa
@Temperature -40.0 °C
34800 psi
@Temperature -40.0 °F
Dry; ISO 604
Shear Strength 65.0 MPa9430 psi3.0% Moisture Content; ASTM D732
 115 MPa16700 psiDry; ASTM D732
Charpy Impact Unnotched  2.50 J/cm²
@Temperature -40.0 °C
11.9 ft-lb/in²
@Temperature -40.0 °F
Dry; ISO 179
 3.00 J/cm²
@Temperature -40.0 °C
14.3 ft-lb/in²
@Temperature -40.0 °F
3.0% Moisture Content; ISO 179
 5.50 J/cm²
@Temperature 23.0 °C
26.2 ft-lb/in²
@Temperature 73.4 °F
Dry; ISO 179
 7.00 J/cm²
@Temperature 23.0 °C
33.3 ft-lb/in²
@Temperature 73.4 °F
3.0% Moisture Content; ISO 179
Charpy Impact, Notched  0.600 J/cm²
@Temperature -40.0 °C
2.86 ft-lb/in²
@Temperature -40.0 °F
V-Notched. Dry; ISO 179
 0.700 J/cm²
@Temperature 23.0 °C
3.33 ft-lb/in²
@Temperature 73.4 °F
V-Notched. Dry; ISO 179
 0.700 J/cm²
@Temperature -40.0 °C
3.33 ft-lb/in²
@Temperature -40.0 °F
V-Notched. 3.0% Moisture Content; ISO 179
 0.850 J/cm²
@Temperature 23.0 °C
4.04 ft-lb/in²
@Temperature 73.4 °F
V-Notched. 3.0% Moisture Content; ISO 179
Coefficient of Friction 0.150.15Vs Metal. Dry. Without lubrication; Suzuki Method
Taber Abrasion, mg/1000 Cycles 0.300.30Dry; ISO 9352
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 1.00e+12 ohm-cm1.00e+12 ohm-cm3.0% Moisture Content; IEC 60093
 1.00e+15 ohm-cm1.00e+15 ohm-cmDry; IEC 60093
Dielectric Constant  3.8
@Frequency 1e+6 Hz
3.8
@Frequency 1e+6 Hz
60% RH; IEC 60250
 4.4
@Frequency 1000 Hz
4.4
@Frequency 1000 Hz
60% RH; IEC 60250
 4.6
@Frequency 50.0 Hz
4.6
@Frequency 50.0 Hz
60% RH; IEC 60250
Dielectric Strength 20.0 kV/mm508 kV/inDry; IEC 60243-1
Dissipation Factor  0.030
@Frequency 1e+6 Hz
0.030
@Frequency 1e+6 Hz
60% RH; IEC 60250
 0.040
@Frequency 50.0 Hz
0.040
@Frequency 50.0 Hz
60% RH; IEC 60250
 0.040
@Frequency 1000 Hz
0.040
@Frequency 1000 Hz
60% RH; IEC 60250
Arc Resistance 120 sec120 secTungsten Electrode. Dry; UL-746A
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 30.0 µm/m-°C16.7 µin/in-°FDry; ISO 11359-2
Specific Heat Capacity 1.60 J/g-°C0.382 BTU/lb-°FDry
Thermal Conductivity 0.330 W/m-K2.29 BTU-in/hr-ft²-°FDry
Melting Point 225 °C437 °FDry; DSC Method
Deflection Temperature at 0.46 MPa (66 psi) 215 °C419 °FDry; ISO 75-1,2
Flammability, UL94  HB
@Thickness 1.60 mm
HB
@Thickness 0.0630 in
3.0% Moisture Content
 HB
@Thickness 1.60 mm
HB
@Thickness 0.0630 in
Dry

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PTORAY9101 / 248791

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.