MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

Huntsman IROGRAN® A 85 P 4394 UV TPU-Polyether
Categories: Polymer; Thermoplastic; Polyurethane, TP; Thermoplastic Polyurethane (TPUR), Polyether Grade

Material Notes: Introduction: IROGRAN A 85 P 4394 is a high performance polyether based thermoplastic polyurethane intended for extrusion and injection molding applications. IROGRAN A 85 P 4394 is part of the HUNTSMAN technical extrusion product range and offers a specially designed, flexible material with a broad processing window particularly suitable for the preparation of tubing, cable jacketing and technical moldings.

Performance Features:

  • High tensile strength
  • Excellent wear performance
  • Excellent hydrolysis & microbial resistance
  • Good low temperature flexibility

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.11 g/cc0.0401 lb/in³injection molded; ASTM D792
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A 8080Injection molded; ASTM D2240
Hardness, Shore D 3030Injection molded; ASTM D2240
Tensile Strength at Break 38.6 MPa5600 psi25 mil film; ASTM D412
Elongation at Break 600 %600 %25 mil film; ASTM D412
100% Modulus 4.69 MPa
@Strain 100 %
680 psi
@Strain 100 %
25 mil film; ASTM D412
300% Modulus 8.27 MPa
@Strain 300 %
1200 psi
@Strain 300 %
25 mil film; ASTM D412
Tear Strength 61.4 kN/m350 pli25 mil film; ASTM D624
Abrasion 3030mm3, injection molded; ISO 4649
 
Thermal PropertiesMetricEnglishComments
Melting Point 145 - 156 °C293 - 313 °FTMA Melt Range, 25 mil film
Vicat Softening Point 69.0 °C
@Load 1.02 kg
156 °F
@Load 2.25 lb
120°C/h, injection molded; ASTM D1525
Oxygen Index 21 %21 %injection molded; ASTM D2863

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Lubrizol ESTANE® ALR CL90A-VE EXP Thermoplastic Polyurethane
Lubrizol Advanced Materials Pearlthane® ECO D12T85 Thermoplastic Polyurethane
Lubrizol Advanced Materials PEARLTHANE® Clear 15N85 Thermoplastic Polyurethane Elastomer
Covestro DUREFLEX® U04 TPU
Huntsman IROGRAN® A 78 E 4723 Polyester-Based TPU-Injection Extrusion Grade

PHUQ121 / 159494

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.