MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

Morgan Advanced Ceramics MACOR® Mac-MGCW Machinable glass ceramic
Categories: Ceramic; Machinable Ceramic

Material Notes: Macor® is the machinable glass ceramic made by Corning Glass and widely used for critically exacting electrical duties. It is a composite of oxides of Si, Mg, Al, K, B and F.

Prime Features:

  • Easily machined into complex shapes and precision components
  • Swift and inexpensive to shape using standard machine tools
  • Vacuum tight
  • Excellent dielectric strength
  • Very high volume resistivity
  • Low thermal conductivity
  • Dimensionally stable
Typical Applications:
  • Vacuum feed-thrus
  • Defense equipment
  • Nuclear related components
Production Capabilities:
  • Distributor of Corning MACOR® in USA and France
  • Wide variety of sizes stocked
  • Machining of simple or complex components to customer specification

Information provided by Morgan Advanced Materials

Key Words: MACOR ®
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Bulk Density 2.52 g/cc0.0910 lb/in³
Open Porosity 0.00 %0.00 %fully dense, apparent
 
Mechanical PropertiesMetricEnglishComments
Hardness, Knoop 250250[kg/mm2]
Modulus of Elasticity 68.0 GPa9860 ksi
Flexural Strength 89.0 MPa12900 psi
Compressive Strength 345 MPa50000 psi
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity  >= 1.00e+14 ohm-cm
@Temperature 25.0 °C
>= 1.00e+14 ohm-cm
@Temperature 77.0 °F
 >= 1.00e+14 ohm-cm
@Temperature 300 °C
>= 1.00e+14 ohm-cm
@Temperature 572 °F
Dielectric Constant 6.03
@Frequency 1e+6 Hz,
Temperature 25.0 °C
6.03
@Frequency 1e+6 Hz,
Temperature 77.0 °F
Dielectric Strength 39.4 kV/mm1000 kV/in
 
Thermal PropertiesMetricEnglishComments
CTE, linear  9.30 µm/m-°C
@Temperature 25.0 - 300 °C
5.17 µin/in-°F
@Temperature 77.0 - 572 °F
 9.30 µm/m-°C
@Temperature 25.0 - 1500 °C
5.17 µin/in-°F
@Temperature 77.0 - 2730 °F
Thermal Conductivity 1.46 W/m-K10.1 BTU-in/hr-ft²-°Fcalculated
Maximum Service Temperature, Air 1000 °C1830 °F
 
Descriptive Properties
Colorwhite

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Corning Macor® Machinable Glass Ceramic
Accuratus MACOR Machinable Glass Ceramic
Aremco AREMCOLOX™ 502-800 Macor® Machinable Glass Ceramic, MGC
Astro Met Macor® Machinable Glass Ceramic
Morgan Advanced Ceramics MACOR® Mac-MGCW Technical Ceramic

CMORF5072 / 200310

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.