MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

Ametek High Purity Nickel Strip 899A 1/4 Hard
Categories: Metal; Nonferrous Metal; Nickel Alloy; Pure Element

Material Notes: Information supplied by Ametek Specialty Metal Products.

AMETEK High Purity Nickel offers major advantages to the rechargeable battery industry, including:

  • Lowest electrical resistivity available in pure nickel strip.
  • Homogeneity, microcleanliness, and close composition control enhances weldability.
  • Significantly low levels of surface oxides reduces die wear and provides excellent solderability.
  • Excellent formability.

Typical applications for rechargeable batteries: computers, cellular phones, power tools, electric vehicles, pagers, and camcorders.

Key Words: Nickel Alloy
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 8.90 g/cc0.322 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell B 70 - 8070 - 80
Hardness, Vickers 120 - 151120 - 151
Tensile Strength, Ultimate 379 - 483 MPa55000 - 70100 psi
Tensile Strength, Yield 172 - 379 MPa
@Strain 0.2 %
24900 - 55000 psi
@Strain 0.2 %
Elongation at Break 20 - 35 %20 - 35 %typical
Poissons Ratio 0.310.31
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.00000763 ohm-cm
@Temperature 20.0 °C
0.00000763 ohm-cm
@Temperature 68.0 °F
Curie Temperature 353 °C667 °F
 
Thermal PropertiesMetricEnglishComments
Thermal Conductivity 86.0 W/m-K
@Temperature 70.0 °C
597 BTU-in/hr-ft²-°F
@Temperature 158 °F
Melting Point 1453 °C2647 °F
 
Component Elements PropertiesMetricEnglishComments
Carbon, C 0.0050 - 0.020 %0.0050 - 0.020 %
Copper, Cu <= 0.0010 %<= 0.0010 %
Iron, Fe <= 0.0050 %<= 0.0050 %
Manganese, Mn <= 0.0010 %<= 0.0010 %
Nickel, Ni >= 99.97 %>= 99.97 %
Silicon, Si <= 0.0010 %<= 0.0010 %
Sulfur, S <= 0.0010 %<= 0.0010 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Nickel, Ni
ATI Allegheny Ludlum AL 200™ Nickel Alloy, UNS N02200

NMA302 / 18196

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.