MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
TSE Industries Millathane® E40 Millable Polyether Polyurethane Rubber, 64A Peroxide Cured Compound
Categories: Polymer; Thermoset; Polyurethane, TS; Thermoset Polyurethane, Elastomer, Unreinforced; Rubber or Thermoset Elastomer (TSE)

Material Notes: Millathane E40 is a sulfur or peroxide curable polyether - TDI polyurethane rubber for the production of rollers, belts seals, gaskets, and other molded parts which require excellent abrasion resistance, low temperature performance, hydrolytic stability and high mechanical strength. Peroxide cure is recommended for best compression set, heat aging, and reversion resistance.

Information provided by TSE Industries

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore A 64
Tensile Strength 20.4 MPa
Elongation at Break 405 %
100% Modulus 0.365 ksi
@Strain 100 %
300% Modulus 1.83 ksi
@Strain 300 %
Resilience 49% Bashore
Tear Strength 24.0 kN/mDie C
Abrasion 79mms loss; DIN Abrasion
Compression Set 14 %
@Temperature 70.0 °C,
Time 79200 sec
 
Processing PropertiesOriginal ValueComments
Cure Time 8.00 min
@Temperature 160 °C
Press Cure, as Tested
 
Descriptive Properties
Formulation as Tested0.5Irganox 1010
 1Structol WB-222
 1SR-350
 10N550 Black
 100Millathane E40
 2Di-Cup 20C
 20N330 Black
 5TP-95

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PMILL9902 / 223016

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.