MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger PEI

(Viewing data as-entered. Click here to return)
Blue Ash Wood
Categories: Wood and Natural Products; Wood; Hardwood

Key Words: Fraxinus Quadrangulata; Lumber, Timber
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 0.530 g/ccGreen, based on volume
 0.580 g/cc12% moisture content, based on volume
 
Mechanical PropertiesOriginal ValueComments
Modulus of Elasticity 1240 ksiGreen
 1400 ksi12% moisture content
Modulus of Rupture 9.60 ksiGreen
 13.8 ksi12% moisture content
Compressive Strength 810 psiGreen, perpendicular to grain
 1420 psi12% moisture content, perpendicular to grain
 4180 psiGreen, parallel to grain
 6980 psi12% moisture content, parallel to grain
Shear Strength 1540 psiGreen, parallel to grain
 2030 psi12% moisture content, parallel to grain
Work to Maximum Load 14.4 in-lb/in³12% moisture content
 14.7 in-lb/in³Green
 
Thermal PropertiesOriginal ValueComments
Shrinkage 3.9 %Radial, from green to oven dry, US origin
 6.5 %Tangential, from green to oven dry, US origin
 11.7 %Volumetric, from green to oven dry, US origin

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Black Wattle Wood
Asian Mengkulang Wood
Balsam Poplar Cottonwood Wood
Berlinia Wood
Bigleaf Hickory Wood

PTSU014 / 71456

Proto3000 – 3D Engineering Solutions

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.