MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

AISI 4419 Steel, double quenched, 230°C (450°F) temper
Categories: Metal; Ferrous Metal; Alloy Steel; AISI 4000 Series Steel; Low Alloy Steel; Carbon Steel; Low Carbon Steel

Material Notes: Carburized 925°C (1700°F) for 8 hrs., pot cooled, reheated to 855°C (1570°F), quenched in agitated oil, reheated to 830°C (1525°F), quenched in agitated oil, 230°C (450°F) temper; 1.8 mm case depth.

Key Words: UNS G44190, ASTM A322, ASTM A331, SAE J404, SAE J412, SAE J770
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 7.85 g/cc0.284 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Brinell 201201
Hardness, Knoop 223223Converted from Brinell
Hardness, Rockwell B 9393Converted from Brinell
Hardness, Rockwell C 1313
Hardness, Vickers 211211Converted from Brinell
Tensile Strength, Ultimate 679 MPa98500 psi
Tensile Strength, Yield 376 MPa54500 psi
Elongation at Break 23.4 %23.4 %in 50 mm.
Reduction of Area 59.7 %59.7 %
Modulus of Elasticity 205 GPa29700 ksiTypical for steel
Bulk Modulus 160 GPa23200 ksiTypical for steel
Poissons Ratio 0.290.29Calculated
Machinability 65 %65 %annealed and cold drawn. Based on 100% machinability for AISI 1212 steel.
Shear Modulus 80.0 GPa11600 ksiTypical for steels.
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.0000245 ohm-cm0.0000245 ohm-cmTypical 4000 series steel
 
Thermal PropertiesMetricEnglishComments
Specific Heat Capacity 0.475 J/g-°C0.114 BTU/lb-°FTypical 4000 series steel
Thermal Conductivity 44.5 W/m-K309 BTU-in/hr-ft²-°FTypical steel
 
Component Elements PropertiesMetricEnglishComments
Carbon, C 0.18 - 0.23 %0.18 - 0.23 %
Iron, Fe 98.095 - 98.77 %98.095 - 98.77 %As remainder
Manganese, Mn 0.45 - 0.65 %0.45 - 0.65 %
Molybdenum, Mo 0.45 - 0.60 %0.45 - 0.60 %
Phosphorus, P <= 0.035 %<= 0.035 %
Silicon, Si 0.15 - 0.35 %0.15 - 0.35 %
Sulfur, S <= 0.040 %<= 0.040 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
AISI 4419 Steel, direct quenched from pot, 150°C (300°F) temper
AISI 4419 Steel, direct quenched from pot, 230°C (450°F) temper
AISI 4419 Steel, double quenched, 150°C (300°F) temper
AISI 4419 Steel, mock carburized, 150°C (300°F) temper, 14 mm (0.55 in.) round
AISI 4419 Steel, mock carburized, 230°C (450°F) temper, 14 mm (0.55 in.) round

M419AS / 7671

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.