MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

Haynes R-41 alloy, 1.27 mm thick sheet, solution heat treated at 1079°C, water quenched, 30 minutes at 1066°C, air cooled, aged 16 hours at 760°C (1400°F)
Categories: Metal; Nonferrous Metal; Nickel Alloy; Superalloy

Material Notes: Vacuum melted, exceptionally high strength at temperature between 649-982°C. Precipitation-hardening type, strength developed by various solutioning and aging heat treatments. Applications include afterburner parts and nozzle diaphragm partitions in current gas turbine engines. Formed with success on drop-hammers, expanding mandrels and stretch formers.

Data provided by the manufacturer, Haynes International, Inc.

Key Words: UNS N07041, AMS 5545, AMS 5712
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 8.25 g/cc0.298 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Ultimate 1047 MPa151900 psi
 179 MPa
@Temperature 982 °C
26000 psi
@Temperature 1800 °F
 677 MPa
@Temperature 871 °C
98200 psi
@Temperature 1600 °F
 858 MPa
@Temperature 760 °C
124000 psi
@Temperature 1400 °F
 958 MPa
@Temperature 538 °C
139000 psi
@Temperature 1000 °F
 970 MPa
@Temperature 649 °C
141000 psi
@Temperature 1200 °F
Tensile Strength, Yield 799 MPa
@Strain 0.2 %
116000 psi
@Strain 0.2 %
 80.0 MPa
@Strain 0.2 %,
Temperature 982 °C
11600 psi
@Strain 0.2 %,
Temperature 1800 °F
 450 MPa
@Strain 0.2 %,
Temperature 871 °C
65300 psi
@Strain 0.2 %,
Temperature 1600 °F
 535 MPa
@Strain 0.2 %,
Temperature 760 °C
77600 psi
@Strain 0.2 %,
Temperature 1400 °F
 746 MPa
@Strain 0.2 %,
Temperature 538 °C
108000 psi
@Strain 0.2 %,
Temperature 1000 °F
 748 MPa
@Strain 0.2 %,
Temperature 649 °C
108000 psi
@Strain 0.2 %,
Temperature 1200 °F
Modulus of Elasticity  150 GPa
@Temperature 927 °C
21800 ksi
@Temperature 1700 °F
 160 GPa
@Temperature 871 °C
23200 ksi
@Temperature 1600 °F
 163 GPa
@Temperature 843 °C
23600 ksi
@Temperature 1550 °F
 166 GPa
@Temperature 816 °C
24100 ksi
@Temperature 1500 °F
 171 GPa
@Temperature 760 °C
24800 ksi
@Temperature 1400 °F
 178 GPa
@Temperature 677 °C
25800 ksi
@Temperature 1250 °F
 179 GPa
@Temperature 649 °C
26000 ksi
@Temperature 1200 °F
 182 GPa
@Temperature 593 °C
26400 ksi
@Temperature 1100 °F
 188 GPa
@Temperature 538 °C
27300 ksi
@Temperature 1000 °F
 190 GPa
@Temperature 482 °C
27600 ksi
@Temperature 900 °F
 198 GPa
@Temperature 371 °C
28700 ksi
@Temperature 700 °F
 204 GPa
@Temperature 260 °C
29600 ksi
@Temperature 500 °F
 213 GPa
@Temperature 149 °C
30900 ksi
@Temperature 300 °F
 218 GPa
@Temperature 25.0 °C
31600 ksi
@Temperature 77.0 °F
Poissons Ratio 0.310.3127°C (80°F)
 0.31
@Temperature 149 °C
0.31
@Temperature 300 °F
 0.32
@Temperature 482 °C
0.32
@Temperature 900 °F
 0.32
@Temperature 371 °C
0.32
@Temperature 700 °F
 0.32
@Temperature 260 °C
0.32
@Temperature 500 °F
 0.33
@Temperature 760 °C
0.33
@Temperature 1400 °F
 0.33
@Temperature 677 °C
0.33
@Temperature 1250 °F
 0.33
@Temperature 649 °C
0.33
@Temperature 1200 °F
 0.34
@Temperature 843 °C
0.34
@Temperature 1550 °F
 0.35
@Temperature 927 °C
0.35
@Temperature 1700 °F
Shear Modulus 83.0 GPa12000 ksi27°C
 55.0 GPa
@Temperature 927 °C
7980 ksi
@Temperature 1700 °F
 61.0 GPa
@Temperature 843 °C
8850 ksi
@Temperature 1550 °F
 64.0 GPa
@Temperature 760 °C
9280 ksi
@Temperature 1400 °F
 67.0 GPa
@Temperature 677 °C
9720 ksi
@Temperature 1250 °F
 69.0 GPa
@Temperature 593 °C
10000 ksi
@Temperature 1100 °F
 72.0 GPa
@Temperature 482 °C
10400 ksi
@Temperature 900 °F
 75.0 GPa
@Temperature 371 °C
10900 ksi
@Temperature 700 °F
 77.0 GPa
@Temperature 260 °C
11200 ksi
@Temperature 500 °F
 81.0 GPa
@Temperature 149 °C
11700 ksi
@Temperature 300 °F
 
Electrical PropertiesMetricEnglishComments
Magnetic Permeability <= 1.002
@Temperature 21.0 °C
<= 1.002
@Temperature 69.8 °F
200 Oersted
 
Thermal PropertiesMetricEnglishComments
CTE, linear  13.5 µm/m-°C
@Temperature 21.0 - 538 °C
7.50 µin/in-°F
@Temperature 69.8 - 1000 °F
 14.0 µm/m-°C
@Temperature 21.0 - 649 °C
7.78 µin/in-°F
@Temperature 69.8 - 1200 °F
 14.8 µm/m-°C
@Temperature 21.0 - 760 °C
8.22 µin/in-°F
@Temperature 69.8 - 1400 °F
 15.2 µm/m-°C
@Temperature 21.0 - 871 °C
8.44 µin/in-°F
@Temperature 69.8 - 1600 °F
 16.3 µm/m-°C
@Temperature 21.0 - 927 °C
9.06 µin/in-°F
@Temperature 69.8 - 1700 °F
 16.8 µm/m-°C
@Temperature 21.0 - 982 °C
9.33 µin/in-°F
@Temperature 69.8 - 1800 °F
Specific Heat Capacity 0.452 J/g-°C
@Temperature 21.0 °C
0.108 BTU/lb-°F
@Temperature 69.8 °F
Thermal Conductivity  11.5 W/m-K
@Temperature 149 °C
79.8 BTU-in/hr-ft²-°F
@Temperature 300 °F
 12.5 W/m-K
@Temperature 204 °C
86.8 BTU-in/hr-ft²-°F
@Temperature 399 °F
 13.6 W/m-K
@Temperature 260 °C
94.4 BTU-in/hr-ft²-°F
@Temperature 500 °F
 14.7 W/m-K
@Temperature 316 °C
102 BTU-in/hr-ft²-°F
@Temperature 601 °F
 16.8 W/m-K
@Temperature 427 °C
117 BTU-in/hr-ft²-°F
@Temperature 801 °F
 18.8 W/m-K
@Temperature 538 °C
130 BTU-in/hr-ft²-°F
@Temperature 1000 °F
 20.0 W/m-K
@Temperature 593 °C
139 BTU-in/hr-ft²-°F
@Temperature 1100 °F
 21.0 W/m-K
@Temperature 644 °C
146 BTU-in/hr-ft²-°F
@Temperature 1190 °F
 22.0 W/m-K
@Temperature 704 °C
153 BTU-in/hr-ft²-°F
@Temperature 1300 °F
 23.1 W/m-K
@Temperature 760 °C
160 BTU-in/hr-ft²-°F
@Temperature 1400 °F
 24.1 W/m-K
@Temperature 816 °C
167 BTU-in/hr-ft²-°F
@Temperature 1500 °F
 25.1 W/m-K
@Temperature 871 °C
174 BTU-in/hr-ft²-°F
@Temperature 1600 °F
Melting Point 1310 - 1345 °C2390 - 2453 °F
Solidus 1310 °C2390 °F
Liquidus 1335 °C2435 °F
 
Component Elements PropertiesMetricEnglishComments
Aluminum, Al 1.4 - 1.6 %1.4 - 1.6 %
Boron, B 0.0030 - 0.010 %0.0030 - 0.010 %
Carbon, C 0.050 - 0.12 %0.050 - 0.12 %
Chromium, Cr 18 - 20 %18 - 20 %
Cobalt, Co 10 - 12 %10 - 12 %
Iron, Fe <= 5.0 %<= 5.0 %
Manganese, Mn <= 0.10 %<= 0.10 %
Molybdenum, Mo 9.0 - 10.5 %9.0 - 10.5 %
Nickel, Ni 53 %53 %As Remainder
Silicon, Si <= 0.50 %<= 0.50 %
Sulfur, S <= 0.015 %<= 0.015 %
Titanium, Ti 3.0 - 3.3 %3.0 - 3.3 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

NHR41O / 17367

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.