MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Chemically Resistant adhesives

Avient Therma-Tech™ ES-5500C TC-EM Polyethersulfone  (discontinued **)
Categories: Polymer; Thermoplastic; Polyethersulfone (PES)

Material Notes:

Description/Features:

  • Thermally Conductive
  • Ceramic Filled
PolyOne First Choice

Information provided by PolyOne Corporation.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.68 g/cc1.68 g/ccASTM D792
Water Absorption 0.10 %
@Thickness 0.508 mm
0.10 %
@Thickness 0.0200 in
24 hr. Immersion; ASTM D570
Linear Mold Shrinkage 0.0039 cm/cm0.0039 in/inASTM D955
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Ultimate 56.5 MPa8190 psiType 1 - Rigids, 0.2 in/min; ASTM D638
Elongation at Break 0.45 %0.45 %Type 1 - Rigids, 0.2 in/min; ASTM D638
Tensile Modulus 26.3 GPa3810 ksiType 1 - Rigids, 0.2 in/min; ASTM D638
Flexural Strength 81.43 MPa11810 psiASTM D790
Flexural Modulus 15.0 GPa2180 ksiASTM D790
Poissons Ratio 0.240.24ASTM E132
Shear Modulus 10.6 GPa1540 ksiCalculated
Izod Impact, Notched 0.214 J/cm
@Thickness 3.17 mm,
Temperature 23.0 °C
0.400 ft-lb/in
@Thickness 0.125 in,
Temperature 73.4 °F
Method A, Injection Molded; ASTM D256
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 6.6 ohm-cm6.6 ohm-cmASTM D257
Dielectric Constant 3.46
@Frequency 1e+6 Hz
3.46
@Frequency 1e+6 Hz
ASTM D150
 
Thermal PropertiesMetricEnglishComments
Thermal Conductivity >= 5.99 W/m-K>= 41.6 BTU-in/hr-ft²-°FASTM C177
Deflection Temperature at 1.8 MPa (264 psi) 196 °C385 °FAnnealed, 0.125 in bars; ASTM D648
 
Descriptive Properties
Product FormPellets

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Gharda Chemicals Gafone™ 3610GM20 Polyethersulfone (PES)
Gharda Chemicals Gafone™ 3100 Polyethersulfone (PES)
Celanese CoolPoly® E3607 Thermally Conductive Polyamide (PA6)
Celanese CoolPoly® E3603 Thermally Conductive Polyphthalamide (PPA)
Celanese CoolPoly® D3612 Thermally Conductive Polyamide (PA66/6)

PH1PO3348 / 45022

Chemically Resistant adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.