Physical Properties | Metric | English | Comments |
---|
Specific Gravity | 1.14 g/cc | 1.14 g/cc |
|
Mechanical Properties | Metric | English | Comments |
---|
Hardness, Shore A | 62 | 62 |
| 50 @Treatment Temp. 23.0 °C, Time 252000 sec | 50 @Treatment Temp. 73.4 °F, Time 70.0 hour |
| 52 @Treatment Temp. 23.0 °C, Time 252000 sec | 52 @Treatment Temp. 73.4 °F, Time 70.0 hour |
| 56 @Treatment Temp. 125 °C, Time 252000 sec | 56 @Treatment Temp. 257 °F, Time 70.0 hour |
| 58 @Treatment Temp. 150 °C, Time 252000 sec | 58 @Treatment Temp. 302 °F, Time 70.0 hour |
| 60 @Treatment Temp. 100 °C, Time 252000 sec | 60 @Treatment Temp. 212 °F, Time 70.0 hour |
| 62 @Treatment Temp. 23.0 °C, Time 252000 sec | 62 @Treatment Temp. 73.4 °F, Time 70.0 hour |
| 62 @Treatment Temp. 100 °C, Time 252000 sec | 62 @Treatment Temp. 212 °F, Time 70.0 hour |
| 62 @Treatment Temp. 125 °C, Time 252000 sec | 62 @Treatment Temp. 257 °F, Time 70.0 hour |
| 62 @Treatment Temp. 100 °C, Time 252000 sec | 62 @Treatment Temp. 212 °F, Time 70.0 hour |
| 64 @Treatment Temp. 150 °C, Time 252000 sec | 64 @Treatment Temp. 302 °F, Time 70.0 hour |
| 65 @Treatment Temp. 100 °C, Time 252000 sec | 65 @Treatment Temp. 212 °F, Time 70.0 hour |
| 69 @Treatment Temp. 125 °C, Time 252000 sec | 69 @Treatment Temp. 257 °F, Time 70.0 hour |
Tensile Strength | 17.3 MPa | 2510 psi |
| 6.092 MPa @Treatment Temp. 23.0 °C, Time 252000 sec | 883.5 psi @Treatment Temp. 73.4 °F, Time 70.0 hour |
| 7.5456 MPa @Treatment Temp. 23.0 °C, Time 252000 sec | 1094.4 psi @Treatment Temp. 73.4 °F, Time 70.0 hour |
| 15.368 MPa @Treatment Temp. 23.0 °C, Time 252000 sec | 2228.9 psi @Treatment Temp. 73.4 °F, Time 70.0 hour |
| 16.856 MPa @Treatment Temp. 150 °C, Time 252000 sec | 2444.7 psi @Treatment Temp. 302 °F, Time 70.0 hour |
| 17.617 MPa @Treatment Temp. 125 °C, Time 252000 sec | 2555.2 psi @Treatment Temp. 257 °F, Time 70.0 hour |
| 18.621 MPa @Treatment Temp. 125 °C, Time 252000 sec | 2700.8 psi @Treatment Temp. 257 °F, Time 70.0 hour |
| 19.054 MPa @Treatment Temp. 125 °C, Time 252000 sec | 2763.5 psi @Treatment Temp. 257 °F, Time 70.0 hour |
| 19.261 MPa @Treatment Temp. 150 °C, Time 252000 sec | 2793.6 psi @Treatment Temp. 302 °F, Time 70.0 hour |
| 19.85 MPa @Treatment Temp. 100 °C, Time 252000 sec | 2879 psi @Treatment Temp. 212 °F, Time 70.0 hour |
| 19.85 MPa @Treatment Temp. 100 °C, Time 252000 sec | 2879 psi @Treatment Temp. 212 °F, Time 70.0 hour |
| 20.162 MPa @Treatment Temp. 100 °C, Time 252000 sec | 2924.2 psi @Treatment Temp. 212 °F, Time 70.0 hour |
Elongation, Ultimate | 432 % | 432 % |
| 167.2 % @Treatment Temp. 23.0 °C, Time 252000 sec | 167.2 % @Treatment Temp. 73.4 °F, Time 70.0 hour |
| 225.1 % @Treatment Temp. 23.0 °C, Time 252000 sec | 225.1 % @Treatment Temp. 73.4 °F, Time 70.0 hour |
| 403.9 % @Treatment Temp. 23.0 °C, Time 252000 sec | 403.9 % @Treatment Temp. 73.4 °F, Time 70.0 hour |
| 413.9 % @Treatment Temp. 125 °C, Time 252000 sec | 413.9 % @Treatment Temp. 257 °F, Time 70.0 hour |
| 431.14 % @Treatment Temp. 125 °C, Time 252000 sec | 431.14 % @Treatment Temp. 257 °F, Time 70.0 hour |
| 432.864 % @Treatment Temp. 150 °C, Time 252000 sec | 432.864 % @Treatment Temp. 302 °F, Time 70.0 hour |
| 434.16 % @Treatment Temp. 125 °C, Time 252000 sec | 434.16 % @Treatment Temp. 257 °F, Time 70.0 hour |
| 442.8 % @Treatment Temp. 150 °C, Time 252000 sec | 442.8 % @Treatment Temp. 302 °F, Time 70.0 hour |
| 447.9 % @Treatment Temp. 100 °C, Time 252000 sec | 447.9 % @Treatment Temp. 212 °F, Time 70.0 hour |
| 457.1 % @Treatment Temp. 100 °C, Time 252000 sec | 457.1 % @Treatment Temp. 212 °F, Time 70.0 hour |
| 457.1 % @Treatment Temp. 100 °C, Time 252000 sec | 457.1 % @Treatment Temp. 212 °F, Time 70.0 hour |
100% Modulus | 1.85 MPa | 268 psi |
Tear Strength | 17.7 kN/m | 101 pli |
| 28.6 kN/m | 163 pli |
Compression Set | 8.7 % @Treatment Temp. 100 °C, Time 79200 sec | 8.7 % @Treatment Temp. 212 °F, Time 22.0 hour |
| 11.6 % @Treatment Temp. 100 °C, Time 79200 sec | 11.6 % @Treatment Temp. 212 °F, Time 22.0 hour |
| 13.7 % @Treatment Temp. 125 °C, Time 79200 sec | 13.7 % @Treatment Temp. 257 °F, Time 22.0 hour |
| 15.1 % @Treatment Temp. 125 °C, Time 79200 sec | 15.1 % @Treatment Temp. 257 °F, Time 22.0 hour |
| 16.4 % @Treatment Temp. 100 °C, Time 252000 sec | 16.4 % @Treatment Temp. 212 °F, Time 70.0 hour |
| 17 % @Treatment Temp. 100 °C, Time 252000 sec | 17 % @Treatment Temp. 212 °F, Time 70.0 hour |
|
Thermal Properties | Metric | English | Comments |
---|
Brittleness Temperature | <= -64.4 °C | <= -84.0 °F |
Shrinkage | -3.10 % @Treatment Temp. 125 °C, Time 252000 sec | -3.10 % @Treatment Temp. 257 °F, Time 70.0 hour |
| -2.90 % @Treatment Temp. 100 °C, Time 252000 sec | -2.90 % @Treatment Temp. 212 °F, Time 70.0 hour |
| -2.90 % @Treatment Temp. 100 °C, Time 252000 sec | -2.90 % @Treatment Temp. 212 °F, Time 70.0 hour |
| 2.4 % @Treatment Temp. 23.0 °C, Time 252000 sec | 2.4 % @Treatment Temp. 73.4 °F, Time 70.0 hour |
| 3.4 % @Treatment Temp. 150 °C, Time 252000 sec | 3.4 % @Treatment Temp. 302 °F, Time 70.0 hour |
| 4.5 % @Treatment Temp. 100 °C, Time 252000 sec | 4.5 % @Treatment Temp. 212 °F, Time 70.0 hour |
| 14.5 % @Treatment Temp. 150 °C, Time 252000 sec | 14.5 % @Treatment Temp. 302 °F, Time 70.0 hour |
| 15.4 % @Treatment Temp. 125 °C, Time 252000 sec | 15.4 % @Treatment Temp. 257 °F, Time 70.0 hour |
| 38 % @Treatment Temp. 23.0 °C, Time 252000 sec | 38 % @Treatment Temp. 73.4 °F, Time 70.0 hour |
| 66.4 % @Treatment Temp. 23.0 °C, Time 252000 sec | 66.4 % @Treatment Temp. 73.4 °F, Time 70.0 hour |
|
Descriptive Properties |
---|
Color | Black |